Phosphor Bronze Wire: Cast Billet Extruded at 570-620 °C, then Cold Drawn without Annealing (Barthel, Lurgi, US 2,079,239)
Charlie

创建者

Charlie

30. 十月 2026DE
4
0
0
0
0

Phosphor Bronze Wire: Cast Billet Extruded at 570-620 °C, then Cold Drawn without Annealing (Barthel, Lurgi, US 2,079,239)

Cast phosphor bronze holds a brittle tin-rich phase that made wire drawing a long round of drawing and annealing. Barthel found that extruding the casting at 570-620 °C kneads it into one soft, even phase, after which it draws straight down to wire. Result: phosphor bronze wire, drawn without intermediate annealing. Source: Barthel, US 2,079,239 (American Lurgi, 1937). His temperature is for about 8 % tin; our ingot has about 9 %, so the same range is ours. Not given: extrusion ratio, die sizes. Picture drawn by Youblob.
高级
2 days

说明

1

Cast a billet and cool it fast

Melt the phosphor bronze and cast it into a billet, cooling it rapidly. Ours: cast in an ingot mould and quench.

此步骤所需材料:

磷青铜锭磷青铜锭1 as required

所需工具:

石墨黏土坩埚石墨黏土坩埚
坩埚炉坩埚炉
锭模锭模
淬火水桶淬火水桶
2

Heat the billet to 570-620 °C

Heat the billet to between about 570 and 620 °C (Barthel's range for about 8 % tin and 0.3 % phosphorus). Temperature: 500-650 °C overall; the less tin, the hotter (about 650 °C for 6 % tin).

所需工具:

马弗炉马弗炉
高温计高温计
3

Extrude it in one pass

Extrude the hot billet in an extrusion press. The kneading makes the metal even all through, practically all alpha. For thick products with little reduction, cold-press the billet 10-20 % first.

所需工具:

液压挤压机液压挤压机
4

Cold draw to wire without annealing

Draw the extruded rod cold through dies down to wire; Barthel's metal needs no annealing between draws. Ours: a steel drawplate with drawing lubricant, one hole smaller each pass.

所需工具:

钢制拉丝板钢制拉丝板
拉丝润滑剂拉丝润滑剂

材料

1

所需工具

9

CC0 公共领域

此蓝图以 CC0 协议发布。你可以自由复制、修改、分发和使用此作品,无需征得许可。

通过购买蓝图中的产品支持创客,他们将获得 创客佣金 (由供应商设定),或创建此蓝图的新版本并将其作为连接包含在你自己的蓝图中以分享收入。

讨论

(0)

登录 加入讨论

加载评论中...