Plaster Bat: a Round Slab Poured in a Frying Pan (Binns, 1910)
Woody

创建者

Woody

4. 十一月 2026NO
5
0
0
0
0

Plaster Bat: a Round Slab Poured in a Frying Pan (Binns, 1910)

A plaster bat is a round slab of plaster that potters use to hold work while making or drying it, and to stiffen wet clay. Binns makes his first one in a frying pan. Variable: plaster per quart of water. 2 3/4 lb is his standard; less gives a softer bat, more a harder one. Source: Charles F. Binns, The Potter's Craft (1910), pp. 43-47. Picture: drawn by Youblob from the text.
初学者
Unknown

说明

1

Make the size

Put a quart of water in a kettle with a piece of soft soap the size of an egg. Simmer about an hour, until the soap has dissolved, and let it cool. Cold, it should be like maple syrup. The size keeps plaster from sticking to a surface.

所需工具:

水水
未知材料未知材料
高壁炖锅高壁炖锅
2

Size the frying pan

Brush size onto the inside of the pan, wipe it off with a sponge, then wash with a second sponge and clean water. On metal one coat often does; repeat until the surface rejects water like grease. On the last coat don't wash: polish with the size sponge. Set the pan on a level table.

所需工具:

碳钢煎锅碳钢煎锅
细毛笔细毛笔
海绵海绵
3

Mix the plaster

Take as much water as fills the pan about 1 in deep; Binns supposes a quart. Weigh 2 3/4 lb of dry potters' plaster for each quart and let it trickle through your fingers into the water in a jug. After about two minutes, when it has soaked up all the water it will take, stir with your hand to a smooth cream, breaking all lumps and removing air bubbles.

此步骤所需材料:

熟石膏熟石膏2.75 磅
水水1 quart

所需工具:

量杯壶量杯壶
秤秤
4

Pour at the right moment

Keep stirring gently until the mix thickens and leaves a white coating on your hand that won't shake off. Then pour it into the pan and shake gently to level it. Poured right, it sets smooth and mat, like sugar icing. Poured too late, it is stiff and hard to level; too soon, it curdles with water on top. Wash the jug at once in a tub, never down a sink: plaster chokes the drain.

所需工具:

碳钢煎锅碳钢煎锅
木盆木盆
5

Turn out and scrape the bat

After about ten minutes the bat grows warm: setting is complete. Hold the pan upside down by the handle and rap its edge smartly on a brick or stone. The disc falls out. Scrape its edge and set it aside. Binns suggests making half a dozen for practice.

所需工具:

碳钢煎锅碳钢煎锅
钢刮刀钢刮刀

材料

2
  • 2.75 磅