PTFE Rod: a Plug Sintered in Boiling Retene Vapour (Brubaker & Hanford 1946)

The first example of du Pont's way to shape PTFE: press a small rod of powder cold, then heat it above 327 °C out of the mould. Here the heat comes from the vapour of boiling retene, which boils at 394 °C, so the temperature holds steady by itself. The plug comes out sintered into one tough piece. Source: M. M. Brubaker and W. E. Hanford (du Pont), US 2,400,099 (1946), Example I. The pressure is the patent's usual range, as the example gives none. The mould, press and the vapour-bath set-up are ours. Picture drawn by Youblob.
高级
1 day

说明

1

Press a plug from the powder

At room temperature, press small particles of PTFE in a mould into a plug 0.5 in across and 0.7 in long. The example gives no pressure; the patent's usual range is 100–3000 lb/sq in.

此步骤所需材料:

PTFE 树脂粉PTFE 树脂粉1 as required for the plug

所需工具:

模压模具模压模具
液压机液压机
直尺直尺
2

Set up a retene vapour bath

Boil retene so its vapour fills the space round a glass tube. Ours: retene in a flask on a burner, a reflux condenser on top, and the tube standing in the vapour.

所需工具:

惹烯惹烯
玻璃蒸馏瓶玻璃蒸馏瓶
回流冷凝管回流冷凝管
本生灯本生灯
试管试管
3

Sinter for 3 hours

Take the plug out of the mould, put it in the glass tube, and heat it in the vapour of boiling retene (394 °C) for 3 hours.

所需工具:

试管试管
惹烯惹烯
本生灯本生灯
4

Cool it under the retene

Remove the heat source and let the plug cool where it is. It is now sintered together into a tough mass.