PTFE Thread Seal Tape: Paste-Extruded, Calendered, Never Sintered
Emma

创建者

Emma

26. 十月 2026SE
10
0
0
0
0

PTFE Thread Seal Tape: Paste-Extruded, Calendered, Never Sintered

The white tape wound on pipe threads is PTFE that has never been melted. Fine PTFE powder is mixed with a lubricant, pressed into a slug, squeezed through a slit die by a ram, rolled thin between two rolls, and dried. Kept below the sintering heat (about 350 °C) it stays soft and conforms to the thread (process: US 5,415,939, 1995). The targets and tests are those of the Indian standard IS 14643 (from BS 4375): no fillers, at most 0.1 % lubricant left, usually 12 mm wide and 0.075 mm thick. The lubricant (naphtha) and the slitter are ours. The picture: Fig. 1a of the patent.
高级
1 day

说明

1

Wet the powder

Mix fine (dispersion-made) virgin PTFE powder with a lubricant that can be driven off completely. Granular PTFE will not paste-extrude. No fillers. Ours: naphtha, as required.

此步骤所需材料:

PTFE 细粉PTFE 细粉1 batch

所需工具:

石脑油石脑油
2

Press a preform

Compact the wet powder into a cylindrical preform in a mould with a plunger.

所需工具:

模压模具模压模具
液压机液压机
3

Ram-extrude a flat tape

Put the preform in the extrusion press. The plunger pushes it out through a slit die as a thick flat tape.

所需工具:

液压挤压机液压挤压机
4

Calender it thin

Pass the tape between two counter-rotating rolls to a thin tape, aiming at about 0.075 mm.

所需工具:

轧机轧机
千分尺千分尺
5

Dry off the lubricant

Dry the tape until the lubricant is gone. Keep it well below the sintering heat (about 350 °C): sintered tape is stiff and will not seal.

所需工具:

干燥炉干燥炉
6

Slit and spool

Slit it to width, usually 12 mm (±0.5 mm), and wind it on spools.

所需工具:

分切复卷机分切复卷机
7

Check the tape

It must look white, with no visible specks or torn edges. Measure the thickness at five points along a sample; each must be within 10 % of their mean.

所需工具:

千分尺千分尺
8

Test the residual lubricant

Weigh about 15 g of tape. Extract it in a Soxhlet with petroleum spirit (40-60 °C) for at least 4 h, dry it at 100 °C, then heat it at 300 °C for 6 h, cool and weigh. The loss must be 0.1 % or less.

所需工具:

索氏提取器索氏提取器
石油醚石油醚
干燥炉干燥炉
钢坩埚钢坩埚
干燥箱(小号)干燥箱(小号)
精密天平精密天平
9

Wrap a thread

Wind tape round an R 1/2 taper pipe thread with 50 % overlap, two layers deep, just tight enough to take the thread form. It must hold the form, not break, and its end must stay put.

所需工具:

螺纹管件螺纹管件

材料

1

所需工具

14

CC0 公共领域

此蓝图以 CC0 协议发布。你可以自由复制、修改、分发和使用此作品,无需征得许可。

通过购买蓝图中的产品支持创客,他们将获得 创客佣金 (由供应商设定),或创建此蓝图的新版本并将其作为连接包含在你自己的蓝图中以分享收入。

讨论

(0)

登录 加入讨论

加载评论中...