Silver Solder from Fine Silver, Copper and Spelter: Gee, 1877
Forge

创建者

Forge

13. 十月 2026NO
14
0
0
0
0

Silver Solder from Fine Silver, Copper and Spelter: Gee, 1877

Silver solder joins silver, copper and brass with a strong, hard seam. The silversmith George Gee preferred one made of fine silver, shot copper and a little spelter (zinc), melted only once: his best hard solder is 16 dwt of fine silver, 3 dwt 12 gr of shot copper and 12 gr of spelter to the ounce, about 80, 17.5 and 2.5 per cent. More copper and zinc make it flow sooner (his medium, easy and common solders). Silver and copper alone give the hardest, least fusible solder; too much zinc makes it eat away during soldering.
中级
Two hours

说明

1

Weigh the metals

正在加载 Jupyter 笔记本…

此步骤所需材料:

纯银纯银80 克
铜锭铜锭17.5 克
锌锭锌锭2.5 克

所需工具:

称重秤称重秤
冷錾冷錾
2

Anneal and test the crucible

Before a new plumbago (graphite) crucible is charged, heat it slowly to redness on a fire that is dying down and has no blaze, so it does not crack. Touch it with a cold iron bar: if cracks show, reject it.

所需工具:

石墨黏土坩埚石墨黏土坩埚
木炭坩埚炉木炭坩埚炉
坩埚钳坩埚钳
3

Melt silver and copper

Put the copper at the bottom of the crucible, the silver on top, and melt them in the furnace. Stir them well together with an iron stirrer, tapered at the point and first heated to redness. When the metals are just beginning to fuse, cover the melt with finely divided, pure charcoal to keep the air off it.

此步骤所需材料:

木炭 - 细磨木炭 - 细磨1 as required

所需工具:

木炭坩埚炉木炭坩埚炉
铁制搅拌棒铁制搅拌棒
耐热手套耐热手套
4

Add the spelter

Hold the spelter in a long pair of tongs over the mouth of the crucible, inside the furnace, until it has almost reached its melting point, then drop it into the molten metal and stir quickly so it mixes in. Zinc burns away quickly in the air, so it goes in last.

所需工具:

火钳火钳
铁制搅拌棒铁制搅拌棒
耐热手套耐热手套
5

Pour the ingot

Withdraw the crucible from the furnace at once and pour into an ingot mould that is clean, smooth, lightly greased, dusted with fine charcoal and warmed: a cold mould makes the metal spout, but do not overheat it either. Melt solder only once; Gee found that solders containing volatile metals grow hard, brittle and drossy with repeated melting.

此步骤所需材料:

木炭 - 细磨木炭 - 细磨1 as required

所需工具:

坩埚钳坩埚钳
锭模锭模
耐热手套耐热手套
6

Roll into pallions or file to dust

Roll the solder out thin between flattening rollers and cut it lengthways and then crossways with hand shears into little bits (pallions), or file it into fine dust, according to the work in hand. The work is then bound together, wetted with a paste of borax and water, and the pallions laid on the joints and melted with a blowpipe flame.

所需工具:

轧机轧机
金属剪金属剪
锉刀(手用锉)锉刀(手用锉)

材料

4
  • 80 克
    占位符
  • 17.5 克
    占位符
  • 2.5 克
    占位符
  • 1 as required
    占位符

所需工具

12

CC0 公共领域

此蓝图以 CC0 协议发布。你可以自由复制、修改、分发和使用此作品,无需征得许可。

通过购买蓝图中的产品支持创客,他们将获得 创客佣金 (由供应商设定),或创建此蓝图的新版本并将其作为连接包含在你自己的蓝图中以分享收入。

讨论

(0)

登录 加入讨论

加载评论中...