Strontium Ferrite Disc Magnet: 0.4 mol SrCO3 to 3.6 mol Iron Oxide, 1270 °C (Went, Philips 1956, Ex. 14)
Charlie

创建者

Charlie

28. 十月 2026DE
1
0
0
0
0

Strontium Ferrite Disc Magnet: 0.4 mol SrCO3 to 3.6 mol Iron Oxide, 1270 °C (Went, Philips 1956, Ex. 14)

A ceramic magnet with strontium in place of barium: 0.4 mol strontium carbonate to 3.6 mol iron oxide, milled 15 hours and passed through a 1270 °C furnace in 20 minutes. Went's rod held 1,290 gauss with a coercive force of 3,080 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 14. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
高级
2 days

说明

1

Weigh strontium carbonate and iron oxide

Weigh 59.1 g strontium carbonate (0.4 mol) and 580.0 g ferric oxide (3.6 mol).

此步骤所需材料:

碳酸锶碳酸锶59.1 克
氧化铁氧化铁580 克

所需工具:

等臂天平等臂天平
P100 防毒面具P100 防毒面具
2

Mill with alcohol 15 hours and dry

Grind with alcohol in a ball mill for 15 hours and dry.

所需工具:

铁球磨机铁球磨机
乙醇——实验级,95 %乙醇——实验级,95 %
干燥炉干燥炉
3

Form the pieces and dry overnight

The patent extrudes rods; ours: press discs at 1.5 tonnes per cm², as in its other examples. Dry overnight.

所需工具:

液压机液压机
圆片压模圆片压模
干燥炉干燥炉
4

Pass through a 1270 °C zone in 20 minutes

Sinter in air at 1270 °C by passing the pieces through a 10 cm hot zone at 5 mm per minute: 20 minutes in the heat.

所需工具:

管式炉管式炉
耐热手套耐热手套
5

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

所需工具:

电磁铁电磁铁
指南针指南针

材料

2

所需工具

11

CC0 公共领域

此蓝图以 CC0 协议发布。你可以自由复制、修改、分发和使用此作品,无需征得许可。

通过购买蓝图中的产品支持创客,他们将获得 创客佣金 (由供应商设定),或创建此蓝图的新版本并将其作为连接包含在你自己的蓝图中以分享收入。

讨论

(0)

登录 加入讨论

加载评论中...