Strontium Ferrite Disc Magnet: Presintered, 4 Minutes at 1150 °C (Went, Philips 1956, Ex. 25)
A strontium ferrite with more strontium: 0.4 mol strontium carbonate to 0.8 mol iron oxide, milled, presintered at 1000 °C, milled again, pressed and passed through a 1150 °C furnace in 4 minutes. Went's rod held 1,200 gauss with a coercive force of 3,710 oersted.
Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 25. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
高级
2 days
说明
1
1
Dry the strontium carbonate and weigh
Dry the strontium carbonate and weigh
Dry the strontium carbonate at 100 °C. Weigh 59.05 g of it (0.4 mol) and 127.5 g ferric oxide (0.8 mol).
此步骤所需材料:
碳酸锶59.05 克
氧化铁127.5 克所需工具:
干燥炉
等臂天平
P100 防毒面具2
2
Mill 7 hours, dry at 110 °C
Mill 7 hours, dry at 110 °C
Grind with alcohol in a ball mill for 7 hours and dry at 110 °C.
所需工具:
铁球磨机
乙醇——实验级,95 %
干燥炉3
3
Presinter in air at 1000 °C for 4 hours
Presinter in air at 1000 °C for 4 hours
Fire in air at 1000 °C for 4 hours.
所需工具:
马弗炉
带盖坩埚(瓷质)
坩埚钳
耐热手套4
4
Mill again, dry, press at 1.5 t/cm²
Mill again, dry, press at 1.5 t/cm²
Grind again 7 hours with alcohol, dry at 110 °C and press at 1.5 tonnes per cm² (ours: discs).
所需工具:
铁球磨机
乙醇——实验级,95 %
干燥炉
液压机
圆片压模5
5
Pass through a 1150 °C zone in 4 minutes
Pass through a 1150 °C zone in 4 minutes
Sinter at 1150 °C by passing the pieces through a 4 cm hot zone at 10 mm per minute: 4 minutes in the heat.
所需工具:
管式炉
耐热手套6
6
Magnetise the discs
Magnetise the discs
The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.