E-glass Fibre Strand: Alkali-Free Lime-Alumina-Borosilicate Glass Drawn to Filament
Charlie

Erstellt von

Charlie

20. Oktober 2026DE
12
0
0
0
0

E-glass Fibre Strand: Alkali-Free Lime-Alumina-Borosilicate Glass Drawn to Filament

Fibre from ordinary glass carries alkali on its huge surface; it takes up water from the air and slowly destroys itself, and it conducts electricity. Schoenlaub's Owens-Corning glass (US 2,334,961, 1943) has no alkali at all: lime, magnesia, alumina and silica fluxed with boric oxide. It was made to be drawn into fibres for insulation and textiles. It is melted at up to 1420 °C and drawn into continuous filaments on a fast spool. The picture: our diagram.
Erfahren
2 days

Anweisungen

1

Weigh out the batch

The patent's example glass: lime (CaO) 17.5 %, magnesia (MgO) 4.5 %, alumina 14.0 %, silica 54.0 %, boric oxide 10.0 %. Ours: weigh those five oxides in those proportions and mix them. Keep within the patent's limits; small changes make this glass devitrify.

Materialien für diesen Schritt:

BranntkalkBranntkalk17.5 parts
MagnesiumoxidMagnesiumoxid4.5 parts
Tonerdepulver (Aluminiumoxid)Tonerdepulver (Aluminiumoxid)14 parts
QuarzsandQuarzsand54 parts
BoroxidBoroxid10 parts

Benötigte Werkzeuge:

BalkenwaageBalkenwaage
SchutzbrilleSchutzbrille
2

Melt at no more than 1420 °C

Melt the batch in a glass tank furnace without going above 1420 °C; the patent's day tanks ran on a 24-hour cycle.

Benötigte Werkzeuge:

GlasschmelzofenGlasschmelzofen
PyrometerPyrometer
Hitzebeständige HandschuheHitzebeständige Handschuhe
SchutzbrilleSchutzbrille
3

Feed the platinum bushing

Draw from a platinum-rhodium bushing like Slayter and Thomas's, heated by an adjustable current. The drawing range of this glass is about 2000–2400 °F (1090–1320 °C). A blower below the nozzles sets each filament.

Benötigte Werkzeuge:

Platin-Rhodium-DüsenwannePlatin-Rhodium-Düsenwanne
AbwärtstransformatorAbwärtstransformator
PyrometerPyrometer
GebläseGebläse
Hitzebeständige HandschuheHitzebeständige Handschuhe
4

Wind on a fast spool

Gather the filaments into a strand and wind it on a spool running as fast as 6,000–10,000 ft per minute (30–50 m/s). Filaments come out about .0001–.0003 in (2.5–7.6 µm) thick. The strand can then be twisted and plied into yarn.

Benötigte Werkzeuge:

AufwickeltrommelAufwickeltrommel

Materialien

5

Benötigte Werkzeuge

9

Dieser Bauplan stellt her

Verwandte Blueprints

Diese Blueprints teilen Wissen — Techniken, Materialien oder Prinzipien

CC0 Gemeinfrei

Dieser Blueprint ist unter CC0 veröffentlicht. Sie dürfen dieses Werk für jeden Zweck frei kopieren, ändern, verbreiten und verwenden, ohne um Erlaubnis zu fragen.

Unterstützen Sie den Maker, indem Sie Produkte über seinen Blueprint kaufen, wo er eine Maker-Provision von Anbietern festgelegt, verdient. Oder erstellen Sie eine neue Iteration dieses Blueprints und verbinden Sie ihn in Ihrem eigenen Blueprint, um Einnahmen zu teilen.

Diskussion

(0)

Anmelden um an der Diskussion teilzunehmen

Kommentare werden geladen...