Spring Steel Strip and Wire, Hardened and Tempered

A spring must bend and come back. Mild steel bends and stays bent; high-carbon steel, hardened and then tempered to a blue colour, springs back. The strip or wire is shaped soft, heated until a magnet no longer sticks to it, quenched in warm oil to harden it, then tempered: cleaned bright and heated gently until the colour runs to blue. It starts from high-carbon crucible steel. Wire is drawn while the steel is still annealed.
Erfahren
A day

Anweisungen

1

Forge strip

Forge crucible steel at a yellow heat into strip, smoothing it with the flatter; never work it below red. Cut it to length while hot.

Materialien für diesen Schritt:

TiegelstahlTiegelstahl1 kg
HolzkohleHolzkohle10 kg

Benötigte Werkzeuge:

SchmiedeesseSchmiedeesse
AmbossAmboss
SchmiedehammerSchmiedehammer
Flachhammer-SetzeisenFlachhammer-Setzeisen
SchmiedezangeSchmiedezange
LederschürzeLederschürze
SchweißerhandschuheSchweißerhandschuhe
SchutzbrilleSchutzbrille
2

Anneal

Heat to a dull red and bury it in dry wood ash to cool slowly overnight.

Materialien für diesen Schritt:

HartholzascheHartholzasche2 kg

Benötigte Werkzeuge:

MetalleimerMetalleimer
3

Draw wire

For wire, forge a rod, anneal it, and draw it through the drawplate with wax, annealing after every hole. Coil or bend the springs now, while it is soft.

Materialien für diesen Schritt:

BienenwachsBienenwachs10 g

Benötigte Werkzeuge:

Zieheisen aus StahlZieheisen aus Stahl
ZiehzangeZiehzange
SchraubstockSchraubstock
4

Harden

Heat the part evenly until a magnet no longer sticks, then plunge it into a lidded bucket of warm rapeseed oil and stir it. Keep the lid at hand for flare-ups.

Materialien für diesen Schritt:

RapsölRapsöl5 Liter

Benötigte Werkzeuge:

SchmiedeesseSchmiedeesse
MagnetMagnet
Metalleimer mit DeckelMetalleimer mit Deckel
SchmiedezangeSchmiedezange
SchweißerhandschuheSchweißerhandschuhe
5

Clean bright

Sand a stripe bright on the hardened steel so you can see the temper colours.

Benötigte Werkzeuge:

SchleifpapierbogenSchleifpapierbogen
6

Temper to blue

Heat it gently and evenly with the torch on fire bricks, or on a hot plate of steel, and watch the colours run straw, bronze, purple, blue. Stop at an even blue and let it cool.

Benötigte Werkzeuge:

PropanbrennerPropanbrenner
SchamottsteinSchamottstein
SchmiedezangeSchmiedezange
7

Test

Clamp one end in the vise and bend the free end a little: it must spring back straight.

Benötigte Werkzeuge:

SchraubstockSchraubstock
Digitaler Messschieber 6 ZollDigitaler Messschieber 6 Zoll
8

Troubleshooting

Spring tempering troubleshooting.

Flow

Loading...

Materialien

5

Benötigte Werkzeuge

18

CC0 Gemeinfrei

Dieser Blueprint ist unter CC0 veröffentlicht. Sie dürfen dieses Werk für jeden Zweck frei kopieren, ändern, verbreiten und verwenden, ohne um Erlaubnis zu fragen.

Unterstützen Sie den Maker, indem Sie Produkte über seinen Blueprint kaufen, wo er eine Maker-Provision von Anbietern festgelegt, verdient. Oder erstellen Sie eine neue Iteration dieses Blueprints und verbinden Sie ihn in Ihrem eigenen Blueprint, um Einnahmen zu teilen.

Diskussion

(0)

Anmelden um an der Diskussion teilzunehmen

Kommentare werden geladen...