Steel Needle: Pointed, Eyed, Hardened in Oil and Tempered
Forge

Creado por

Forge

18. octubre 2026NO
16
0
0
0
0

Steel Needle: Pointed, Eyed, Hardened in Oil and Tempered

Needles are made from good steel wire: cut, straightened, pointed, flattened and pierced for the eye, hardened by heating and plunging into oil, then tempered back to a springy hardness, scoured and polished (Bucknall Smith, A Treatise upon Wire, 1891). This is the same sequence by hand, one heavy needle at a time from piano wire; the hand methods and sizes are ours. The picture: steel sewing needles (Wikimedia Commons).
Intermedio
Half a day

Instrucciones

1

Cut, soften and straighten

Cut 70 mm of 1.2 mm piano wire. Heat it to red in the forge and let it cool slowly in the ashes so it can be filed and drilled, then roll it straight on the anvil.

Materiales para este paso:

Cuerda de pianoCuerda de piano70 mm

Herramientas necesarias:

Alicates de corteAlicates de corte
Fragua de herreroFragua de herrero
Alicates de punta finaAlicates de punta fina
YunqueYunque
2

Point

Clamp it in the vise and file a long, even taper to a sharp point, turning the wire as you go.

Herramientas necesarias:

Juego de limasJuego de limas
Tornillo de bancoTornillo de banco
Gafas de seguridadGafas de seguridad
3

Flatten and pierce the eye

Flatten the head end slightly on the anvil, drill the eye through the flat with the finest bit, then file off the burrs and round the head.

Herramientas necesarias:

YunqueYunque
Martillo de peña transversalMartillo de peña transversal
Taladro de manoTaladro de mano
Juego de limasJuego de limas
Tornillo de bancoTornillo de banco
Gafas de seguridadGafas de seguridad
4

Harden in oil

Heat the needle evenly to red and plunge it into the oil. It is now glass-hard and brittle.

Herramientas necesarias:

Fragua de herreroFragua de herrero
Alicates de punta finaAlicates de punta fina
Cubeta de temple con aceiteCubeta de temple con aceite
Gafas de seguridadGafas de seguridad
5

Temper

Reheat it in the oven to about 600 °F (315 °C) and let it cool slowly to a springy temper. If it came out crooked, straighten it with light blows of a small hammer on the anvil.

Herramientas necesarias:

Horno de tratamiento térmicoHorno de tratamiento térmico
Termopar con indicadorTermopar con indicador
YunqueYunque
Martillo de peña transversalMartillo de peña transversal
6

Scour and polish

Scour it bright with emery cloth, a little oil and soap. Wash it in hot water, dry it in sawdust, touch up the point, and polish it on the leather strop.

Herramientas necesarias:

Tela de esmerilTela de esmeril
Aceite de olivaAceite de oliva
JabónJabón
SerrínSerrín
Asentador de cueroAsentador de cuero
Juego de limasJuego de limas

Materiales

1

Herramientas requeridas

17

CC0 Dominio público

Este Blueprint se publica bajo CC0. Eres libre de copiar, modificar, distribuir y usar este trabajo para cualquier propósito, sin pedir permiso.

Apoya al Maker comprando productos a través de su Blueprint, donde gana una Comisión del Maker establecida por los vendedores, o crea una nueva iteración de este Blueprint e inclúyela como conexión en tu propio Blueprint para compartir ingresos.

Discusión

(0)

Iniciar sesión para unirte a la discusión

Cargando comentarios...