Barium-Calcium Ferrite Disc Magnet: 20 % Calcium, 5 Minutes at 1290 °C (Went, Philips 1956, Ex. 20)
A ceramic magnet with a fifth of the barium replaced by calcium: 0.08 mol barium carbonate, 0.02 mol calcium carbonate and 0.6 mol iron oxide, made as in Example 18 but sintered at 1290 °C for only 5 minutes. Went's rod held 1,615 gauss with a coercive force of 1,550 oersted.
Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 20. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Avancé
2 days
Consignes
1
1
Weigh barium carbonate, chalk and iron oxide
Weigh barium carbonate, chalk and iron oxide
Weigh 15.79 g barium carbonate (0.08 mol), 2.002 g calcium carbonate (0.02 mol) and 95.55 g ferric oxide (0.6 mol). Barium carbonate is poisonous if swallowed: gloves and a dust respirator.
Matériaux pour cette étape :
Carbonate de baryum (withérite)15.79 g
Carbonate de calcium (blanc de Meudon)2.002 g
Oxyde ferrique95.55 gOutils nécessaires :
Balance à fléau
Gants en caoutchouc
Masque respiratoire P1002
2
Mill, presinter and mill as in Example 18
Mill, presinter and mill as in Example 18
As in Example 18: grind with alcohol 4 hours, dry at 150 °C, fire in air at 1000 °C for 2 hours, grind again 4 hours and dry.
Outils nécessaires :
Broyeur à boulets de fer
Éthanol de laboratoire, 95 %
Étuve de séchage
Four à moufle
Creuset avec couvercle (porcelaine)
Pince à creuset3
3
Press at 1.5 t/cm²
Press at 1.5 t/cm²
Press at 1.5 tonnes per cm², as in Example 18 (ours: discs instead of rods).
Outils nécessaires :
Presse hydraulique
Matrice de pressage de disques4
4
Pass through a 1290 °C zone in 5 minutes
Pass through a 1290 °C zone in 5 minutes
Sinter in air at 1290 °C by passing the pieces through a 10 cm hot zone at 20 mm per minute: 5 minutes in the heat.
Outils nécessaires :
Four tubulaire
Gants résistants à la chaleur5
5
Magnetise the discs
Magnetise the discs
The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.
Outils nécessaires :
Électroaimant
BoussoleMatériaux
3- Espace réservé
- Espace réservé
- 95.55 gEspace réservé
Outils requis
15- Espace réservé
- Espace réservé
- Espace réservé
- Espace réservé
- Espace réservé
- Espace réservé
- Espace réservé
- Espace réservé
- Espace réservé
- Espace réservé
- Espace réservé
- Espace réservé
- Espace réservé
- Espace réservé
- Espace réservé
Ce plan fabrique
Blueprints liés
Ces blueprints partagent des connaissances — techniques, matériaux ou principes
CC0 Domaine public
Ce blueprint est publié sous CC0. Vous êtes libre de copier, modifier, distribuer et utiliser ce travail pour tout usage, sans demander la permission.