Barium Ferrite Disc Magnet: Barium Carbonate and Iron Oxide Sintered (Went, Philips 1956)
The dark grey ceramic magnet on fridges and in loudspeakers is barium ferrite. It is made from two cheap powders: one part barium carbonate to six of iron oxide, milled, fired, milled again, pressed and sintered. No cobalt or nickel is needed. This is Example 34 of the Philips patent. Fired 4 hours at 1100 °C, its rod held 1,375 gauss with a coercive force of 3,350 oersted.
Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956). They pressed rods; the claim covers "a body of a desired shape", and the disc size is ours. The patent does not say how to magnetise it; our way is stated. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Avancé
2 days
Consignes
1
1
Weigh one part barium carbonate to six of iron oxide
Weigh one part barium carbonate to six of iron oxide
Weigh 39.5 g of barium carbonate (0.2 mol) and 191.7 g of ferric oxide, Fe2O3 (1.2 mol). Barium carbonate is poisonous if swallowed: ours, gloves and a dust respirator.
Matériaux pour cette étape :
Carbonate de baryum (withérite)39.5 g
Oxyde ferrique191.7 gOutils nécessaires :
Balance à fléau
Gants en caoutchouc
Masque respiratoire P1002
2
Mill with ethanol for 4 hours
Mill with ethanol for 4 hours
Grind the mixture with ethanol in an iron ball mill for 4 hours. Let the ethanol evaporate, then dry the powder in a drying oven.
Outils nécessaires :
Broyeur à boulets de fer
Éthanol de laboratoire, 95 %
Étuve de séchage3
3
Presinter at 1000 °C for 4 hours
Presinter at 1000 °C for 4 hours
Fire the dry powder in air at 1000 °C for 4 hours (ours: in a lidded porcelain crucible in a muffle furnace). Let it cool.
Outils nécessaires :
Four à moufle
Creuset avec couvercle (porcelaine)
Pince à creuset
Gants résistants à la chaleur4
4
Mill again for 4 hours
Mill again for 4 hours
Grind the presintered product with ethanol in the ball mill for another 4 hours. Let the ethanol evaporate.
Outils nécessaires :
Broyeur à boulets de fer
Éthanol de laboratoire, 95 %
Étuve de séchage
Masque respiratoire P1005
5
Press discs at 1.5 tons per cm²
Press discs at 1.5 tons per cm²
Press the powder at 1.5 tons/cm². The patent pressed rods; we press discs. Ours: a die 20 mm across, so about 4.7 tonnes on the punch (our arithmetic: 1.5 × 3.14 cm²).
Outils nécessaires :
Presse hydraulique
Matrice de pressage de disques6
6
Sinter for 4 hours
Sinter for 4 hours
Sinter the discs for 4 hours in oxygen or in air. The patent's results: at 1100 °C, 1,375 gauss and 3,350 oersted; at 1200 °C, 1,400 and 3,100; at 1300 °C, 1,850 and 1,780. Hotter gives a stronger but less stubborn magnet.
Outils nécessaires :
Four à moufle
Pince à creuset
Gants résistants à la chaleur7
7
Magnetise the discs
Magnetise the discs
The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.
Outils nécessaires :
Électroaimant
BoussoleMatériaux
2- Espace réservé
- 191.7 gEspace réservé
Outils requis
14- Espace réservé
- Espace réservé
- Espace réservé
- Espace réservé
- Espace réservé
- Espace réservé
- Espace réservé
- Espace réservé
- Espace réservé
- Espace réservé
- Espace réservé
- Espace réservé
- Espace réservé
- Espace réservé
Ce plan fabrique
Blueprints liés
Ces blueprints partagent des connaissances — techniques, matériaux ou principes
CC0 Domaine public
Ce blueprint est publié sous CC0. Vous êtes libre de copier, modifier, distribuer et utiliser ce travail pour tout usage, sans demander la permission.
Soutenez le Maker en achetant des produits via son Blueprint où il perçoit une Commission Maker définie par les Vendeurs, ou créez une nouvelle itération de ce Blueprint et incluez-le comme connexion dans votre propre Blueprint pour partager les revenus.