Barium-Calcium Ferrite Disc Magnet: Equal Barium and Calcium, Sintered at 1280 °C (Went, Philips 1956, Ex. 22)
Charlie

Créé par

Charlie

28. octobre 2026DE
1
0
0
0
0

Barium-Calcium Ferrite Disc Magnet: Equal Barium and Calcium, Sintered at 1280 °C (Went, Philips 1956, Ex. 22)

A ceramic magnet with equal parts barium and calcium: 0.3 mol barium carbonate, 0.3 mol calcium carbonate and 3.1 mol iron oxide, milled 15 hours, pressed and passed through a 1280 °C furnace in 10 minutes, with no presintering. Went's rod held 1,595 gauss with a coercive force of 1,890 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 22. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Avancé
2 days

Consignes

1

Weigh barium carbonate, chalk and iron oxide

Weigh 59.5 g barium carbonate (0.3 mol), 30.2 g calcium carbonate (0.3 mol) and 500.0 g ferric oxide (3.1 mol). Barium carbonate is poisonous if swallowed: gloves and a dust respirator.

Matériaux pour cette étape :

Carbonate de baryum (withérite)Carbonate de baryum (withérite)59.5 g
Carbonate de calcium (blanc de Meudon)Carbonate de calcium (blanc de Meudon)30.2 g
Oxyde ferriqueOxyde ferrique500 g

Outils nécessaires :

Balance à fléauBalance à fléau
Gants en caoutchoucGants en caoutchouc
Masque respiratoire P100Masque respiratoire P100
2

Mill with alcohol 15 hours, dry, press

Grind with alcohol in a ball mill for 15 hours, dry, and press at 1.5 tonnes per cm² (ours: discs instead of rods). No presintering.

Outils nécessaires :

Broyeur à boulets de ferBroyeur à boulets de fer
Éthanol de laboratoire, 95 %Éthanol de laboratoire, 95 %
Étuve de séchageÉtuve de séchage
Presse hydrauliquePresse hydraulique
Matrice de pressage de disquesMatrice de pressage de disques
3

Pass through a 1280 °C zone in 10 minutes

Sinter at 1280 °C by passing the pieces through a 10 cm hot zone at 10 mm per minute: 10 minutes in the heat.

Outils nécessaires :

Four tubulaireFour tubulaire
Gants résistants à la chaleurGants résistants à la chaleur
4

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

Outils nécessaires :

ÉlectroaimantÉlectroaimant
BoussoleBoussole

Matériaux

3

Outils requis

12

Blueprints liés

Ces blueprints partagent des connaissances — techniques, matériaux ou principes

CC0 Domaine public

Ce blueprint est publié sous CC0. Vous êtes libre de copier, modifier, distribuer et utiliser ce travail pour tout usage, sans demander la permission.