Barium Ferrite Disc Magnet from Natural Magnetite, Presintered at 900 °C (Went, Philips 1956, Ex. 36, Procedure 1)
A barium ferrite magnet made from natural magnetite instead of ferric oxide: barium carbonate and magnetite ground 18 hours, presintered 3 hours at 900 °C, ground again 18 hours, pressed and sintered 2 hours at 1200 °C. Went's rod held 1,450 gauss with a coercive force of 2,425 oersted.
Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 36. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Avancé
2 days
Consignes
1
1
Weigh barium carbonate and magnetite
Weigh barium carbonate and magnetite
Weigh 9.9 g barium carbonate (0.05 mol) and 46.9 g natural magnetite, Fe3O4 (0.20 mol). Barium carbonate is poisonous if swallowed: gloves and a dust respirator.
Matériaux pour cette étape :
Carbonate de baryum (withérite)9.9 g
Magnétite46.9 gOutils nécessaires :
Balance à fléau
Gants en caoutchouc
Masque respiratoire P1002
2
Grind 18 hours in a ball mill
Grind 18 hours in a ball mill
Grind the mixture in a ball mill for 18 hours. The patent does not say whether wet or dry.
Outils nécessaires :
Broyeur à boulets de fer
Masque respiratoire P1003
3
Presinter at 900 °C for 3 hours
Presinter at 900 °C for 3 hours
Fire the ground mixture at 900 °C for three hours and let it cool.
Outils nécessaires :
Four à moufle
Creuset avec couvercle (porcelaine)
Pince à creuset
Gants résistants à la chaleur4
4
Grind 18 hours in a ball mill
Grind 18 hours in a ball mill
Grind it again in a ball mill for 18 hours. The patent does not say whether wet or dry.
Outils nécessaires :
Broyeur à boulets de fer
Masque respiratoire P1005
5
Press at 1.5 t/cm²
Press at 1.5 t/cm²
Press at 1.5 tonnes per cm² (ours: discs instead of a rod).
Outils nécessaires :
Presse hydraulique
Matrice de pressage de disques6
6
Sinter at 1200 °C for 2 hours
Sinter at 1200 °C for 2 hours
Sinter at 1200 °C for 2 hours. The patent gives no atmosphere for this example. Went's rod: 1,450 gauss, 2,425 oersted.
Outils nécessaires :
Four à moufle
Pince à creuset
Gants résistants à la chaleur7
7
Magnetise the discs
Magnetise the discs
The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.
Outils nécessaires :
Électroaimant
BoussoleOutils requis
12- Espace réservé
- Espace réservé
- Espace réservé
- Espace réservé
- Espace réservé
- Espace réservé
- Espace réservé
- Espace réservé
- Espace réservé
- Espace réservé
- Espace réservé
- Espace réservé
Ce plan fabrique
Blueprints liés
Ces blueprints partagent des connaissances — techniques, matériaux ou principes
CC0 Domaine public
Ce blueprint est publié sous CC0. Vous êtes libre de copier, modifier, distribuer et utiliser ce travail pour tout usage, sans demander la permission.
Soutenez le Maker en achetant des produits via son Blueprint où il perçoit une Commission Maker définie par les Vendeurs, ou créez une nouvelle itération de ce Blueprint et incluez-le comme connexion dans votre propre Blueprint pour partager les revenus.