ART
BEAUTÉ ET BIEN-ÊTRE
ARTISANAT
CULTURE ET HISTOIRE
DIVERTISSEMENT
ENVIRONNEMENT
NOURRITURE ET BOISSONS
INGÉNIERIE INVERSE
SCIENCES
SPORTS
TECHNOLOGIE
TECHNOLOGIE PORTABLE
Barium Ferrite Disc Magnet from Natural Magnetite, Pressed Without Presintering (Went, Philips 1956, Ex. 36, Procedure 2)
Charlie

Créé par

Charlie

28. octobre 2026DE
1
0
0
0
0

Barium Ferrite Disc Magnet from Natural Magnetite, Pressed Without Presintering (Went, Philips 1956, Ex. 36, Procedure 2)

A barium ferrite magnet from barium carbonate and natural magnetite, ground 18 hours and pressed straight away, with no presintering, then sintered 2 hours at 1200 °C. Went's rod held 1,520 gauss with a coercive force of 2,385 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 36. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Avancé
2 days

Consignes

1

Weigh barium carbonate and magnetite

Weigh 9.9 g barium carbonate (0.05 mol) and 46.9 g natural magnetite, Fe3O4 (0.20 mol). Barium carbonate is poisonous if swallowed: gloves and a dust respirator.

Matériaux pour cette étape :

Carbonate de baryum (withérite)Carbonate de baryum (withérite)9.9 g
MagnétiteMagnétite46.9 g

Outils nécessaires :

Balance à fléauBalance à fléau
Gants en caoutchoucGants en caoutchouc
Masque respiratoire P100Masque respiratoire P100
2

Grind 18 hours in a ball mill

Grind the mixture in a ball mill for 18 hours. The patent does not say whether wet or dry.

Outils nécessaires :

Broyeur à boulets de ferBroyeur à boulets de fer
Masque respiratoire P100Masque respiratoire P100
3

Press at 1.5 t/cm²

Press at 1.5 tonnes per cm² (ours: discs instead of a rod).

Outils nécessaires :

Presse hydrauliquePresse hydraulique
Matrice de pressage de disquesMatrice de pressage de disques
4

Sinter at 1200 °C for 2 hours

Sinter at 1200 °C for 2 hours. The patent gives no atmosphere for this example. Went's rod: 1,520 gauss, 2,385 oersted.

Outils nécessaires :

Four à moufleFour à moufle
Pince à creusetPince à creuset
Gants résistants à la chaleurGants résistants à la chaleur
5

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

Outils nécessaires :

ÉlectroaimantÉlectroaimant
BoussoleBoussole

Matériaux

2

Outils requis

11

Blueprints liés

Ces blueprints partagent des connaissances — techniques, matériaux ou principes

CC0 Domaine public

Ce blueprint est publié sous CC0. Vous êtes libre de copier, modifier, distribuer et utiliser ce travail pour tout usage, sans demander la permission.

Soutenez le Maker en achetant des produits via son Blueprint où il perçoit une Commission Maker définie par les Vendeurs, ou créez une nouvelle itération de ce Blueprint et incluez-le comme connexion dans votre propre Blueprint pour partager les revenus.

Commentaires

(0)

Se connecter pour participer à la discussion

Chargement des commentaires...