Barium Ferrite Disc Magnet: 0.5 mol BaCO3 to 3.5 mol Iron Oxide, 10 Minutes at 1330 °C (Went, Philips 1956, Ex. 4)
Charlie

Créé par

Charlie

28. octobre 2026DE
1
0
0
0
0

Barium Ferrite Disc Magnet: 0.5 mol BaCO3 to 3.5 mol Iron Oxide, 10 Minutes at 1330 °C (Went, Philips 1956, Ex. 4)

A barium ferrite with much more iron oxide: 0.5 mol barium carbonate to 3.5 mol, milled 15.5 hours, bound, formed and sintered 10 minutes at 1330 °C. Went's rod held 2,040 gauss with a coercive force of 2,380 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 4. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Avancé
2 days

Consignes

1

Weigh barium carbonate and iron oxide

Weigh 99.2 g barium carbonate (0.5 mol) and 564.8 g ferric oxide (3.5 mol). Barium carbonate is poisonous if swallowed: gloves and a dust respirator.

Matériaux pour cette étape :

Carbonate de baryum (withérite)Carbonate de baryum (withérite)99.2 g
Oxyde ferriqueOxyde ferrique564.8 g

Outils nécessaires :

Balance à fléauBalance à fléau
Gants en caoutchoucGants en caoutchouc
Masque respiratoire P100Masque respiratoire P100
2

Mill with alcohol 15.5 hours, dry and sieve

Grind the mixture with alcohol in a ball mill for 15.5 hours, then dry it and sieve it.

Outils nécessaires :

Broyeur à boulets de ferBroyeur à boulets de fer
Éthanol de laboratoire, 95 %Éthanol de laboratoire, 95 %
Étuve de séchageÉtuve de séchage
CribleCrible
3

Knead with a binder and form

Mix 300 g of the powder with a binder such as polyvinyl alcohol (Went names it or nitrocellulose) into a kneadable mass. The patent extrudes rods about 3 mm across; ours: press discs at 1.5 tonnes per cm², as in its other examples. Dry them in air for about 24 hours.

Outils nécessaires :

Alcool polyvinylique en poudreAlcool polyvinylique en poudre
Presse hydrauliquePresse hydraulique
Matrice de pressage de disquesMatrice de pressage de disques
Étuve de séchageÉtuve de séchage
4

Sinter in air at 1330 °C for 10 minutes

Sinter the pieces in air at 1330 °C for 10 minutes. The patent gives no zone length or speed for this example.

Outils nécessaires :

Four tubulaireFour tubulaire
Gants résistants à la chaleurGants résistants à la chaleur
5

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

Outils nécessaires :

ÉlectroaimantÉlectroaimant
BoussoleBoussole

Matériaux

2

Outils requis

14

Blueprints liés

Ces blueprints partagent des connaissances — techniques, matériaux ou principes

CC0 Domaine public

Ce blueprint est publié sous CC0. Vous êtes libre de copier, modifier, distribuer et utiliser ce travail pour tout usage, sans demander la permission.

Soutenez le Maker en achetant des produits via son Blueprint où il perçoit une Commission Maker définie par les Vendeurs, ou créez une nouvelle itération de ce Blueprint et incluez-le comme connexion dans votre propre Blueprint pour partager les revenus.

Commentaires

(0)

Se connecter pour participer à la discussion

Chargement des commentaires...