Epoxy Resin

Pierre Castan, a Swiss chemist at the dental firm De Trey Frères, was looking for a resin for dentures. He reacted a phenol carrying two hydroxy groups with epichlorohydrin, then hardened the product with an acid anhydride, and got a hard, clear, unusually adherent solid. Ciba licensed it and sold it as Araldite; in the US Sylvan Greenlee developed epoxies independently. **US 2,324,483**, "Process of preparing synthetic resins", Castan, granted 20. July 1943, claims condensing "a polybasic carboxylic acid anhydride" with the product of "a phenol having at least two phenolic hydroxy groups and of an epichlorhydrine". It does not single out bisphenol A, the phenol most epoxies use today. **Epichlorohydrin is a carcinogen; you start from a two-part kit.** You glue pine lap joints at the right ratio and four wrong ones, then test hardness and break the joints.
Débutant
2 hours plus 24 h cure

Consignes

1

Cut the joint pieces

Saw ten pine strips 100 x 25 mm. Sand one face of each end with 120 grit and dust off. Label five pairs 1:1, 1.25:1, 1:1.25, 1.5:1 and 1:1.5.

Matériaux pour cette étape :

Planche de pinPlanche de pin1 pièce
Papier abrasifPapier abrasif1 feuille
Ruban de masquageRuban de masquage1 rouleau

Outils nécessaires :

Scie égoïneScie égoïne
Règle en acierRègle en acier
CrayonCrayon
2

Measure by syringe

Gloves on. For each ratio draw resin and hardener in separate syringes (1:1 = 2 ml + 2 ml; 1.25:1 = 2.5 + 2; and so on) into its own cup. This assumes a 1:1-by-volume kit - scale to your label.

Matériaux pour cette étape :

Époxy à deux composantsÉpoxy à deux composants25 ml

Outils nécessaires :

Gants en nitrileGants en nitrile
Jeu de seringuesJeu de seringues
Gobelets gradués de mélangeGobelets gradués de mélange
Lunettes de sécurité transparentesLunettes de sécurité transparentes
3

Mix thoroughly

Stir each cup 2 minutes, scraping the walls and bottom. Unmixed streaks behave like a wrong ratio.

Outils nécessaires :

Baguette d'agitationBaguette d'agitation
4

Glue and pour

Spread each mix on the sanded ends of its pair, overlap them 25 mm and spring-clamp over wax paper. Pour the rest as a coin-sized puddle on wax paper beside it.

Matériaux pour cette étape :

Papier sulfuriséPapier sulfurisé1 feuille

Outils nécessaires :

Serre-joint à ressortSerre-joint à ressort
5

Cure 24 hours

Leave everything at room temperature, 20 °C or warmer, for 24 hours. Cold slows the cure.
6

Pencil hardness

Sharpen pencils 6B to 6H and flatten the tips on 400 grit. Push each at 45° across a puddle, from hard down, until one no longer scratches. Record that grade.

Outils nécessaires :

Jeu de crayons graphiteJeu de crayons graphite
Loupe de bijoutierLoupe de bijoutier
7

Break the joints

Clamp one strip of a joint in the vise and tap the free end sideways with the mallet until it breaks. Estimate how much of the bond face is torn wood.

Outils nécessaires :

Étau d'établiÉtau d'établi
Maillet en caoutchoucMaillet en caoutchouc
Lunettes de sécurité transparentesLunettes de sécurité transparentes
8

Ratio, leftovers, results

Chargement du notebook Jupyter…
9

History & Context

**What the patent specifies:** a resin from a two-hydroxy phenol and epichlorohydrin, hardened by a polybasic acid anhydride. **Modern build (derived):** a two-part kit, most with an amine hardener that cures at room temperature. Epoxy became the glue that holds metal, the matrix of fibreglass and carbon-fibre parts, and the boat-builder's resin. Its limits: it yellows in sunlight, softens with heat, and uncured resin and hardener sensitise skin - which is why the gloves stay on every time.

Matériaux

5

Outils requis

13

CC0 Domaine public

Ce blueprint est publié sous CC0. Vous êtes libre de copier, modifier, distribuer et utiliser ce travail pour tout usage, sans demander la permission.

Soutenez le Maker en achetant des produits via son Blueprint où il perçoit une Commission Maker définie par les Vendeurs, ou créez une nouvelle itération de ce Blueprint et incluez-le comme connexion dans votre propre Blueprint pour partager les revenus.

Commentaires

(0)

Se connecter pour participer à la discussion

Chargement des commentaires...