Smith's Fire Rake (Poker): a 3/8 in. Rod Drawn to a Flat Point, Crooked, and Looped Over the Anvil (Edwinson, 1886)
Forge

Créé par

Forge

14. novembre 2026NO
9
0
0
0
0

Smith's Fire Rake (Poker): a 3/8 in. Rod Drawn to a Flat Point, Crooked, and Looped Over the Anvil (Edwinson, 1886)

The first job George Edwinson set his readers in Amateur Work (1886): the smith's rake for the forge fire, which "might be dubbed a poker". A yard of 3/8 in. iron rod drawn to a square then flat point with quarter turns, bent into a crook, and the other end bent round in three heats into a loop handle.
Débutant
An hour at the forge

Consignes

1

His sizes

Chargement du notebook Jupyter…
2

Read Edwinson

"The rake, Fig. 16, might be dubbed a poker, and as this is the most simple tool, we will deal with that first."
3

Light a small fire

Pile slack round the tuyere, scoop a shallow pit in front of it, put in shavings with a few cinders on top, light and blow gently. Draw slack in until the heap glows, then damp the outside so the fire stays within 6 in. (15 cm) of the tuyere.

Matériaux pour cette étape :

Charbon bitumineuxCharbon bitumineux1 pièce

Outils nécessaires :

Forge de forgeronForge de forgeron
4

Draw the point

Cut 36 in. (91 cm) of 3/8 in. (10 mm) iron rod with a cold chisel. Heat 2 in. of one end glowing white. On the outer edge of the anvil, hammer it lightly on the tip, giving the rod a quarter turn after each blow and drawing it back, to a square point. Strike only while it glows; reheat at a dull red. Next heat, round the corners and draw a flat tapering point (fig. 17).

Matériaux pour cette étape :

Barre de fer forgéBarre de fer forgé1 pièce

Outils nécessaires :

Burin à froidBurin à froid
Forge de forgeronForge de forgeron
EnclumeEnclume
MarteauMarteau
5

Crook the end

Heat the point to a dull red and bend it over the outer edge of the anvil with a few light blows into the crook (fig. 16).

Outils nécessaires :

Forge de forgeronForge de forgeron
EnclumeEnclume
MarteauMarteau
6

Bend the loop

Heat the rod about 10 in. from the other end to redness and bend it over the anvil edge (fig. 18). Heat 3 in. more of the bent part and shape it (fig. 19). Heat again and bring the end round to touch the shoulder (fig. 20), then shape the loop hot with light blows. (Experienced smiths scarf the end and weld it to the shoulder.)

Outils nécessaires :

Forge de forgeronForge de forgeron
EnclumeEnclume
MarteauMarteau
7

Troubleshooting

Rake troubleshooting.

Flow

Loading...
8

History and honest limits

From George Edwinson, "Smithing and Forging" II, **Amateur Work, Illustrated**, vol. V (1886), pp. 211-213 and figs. 15-20 (checked on the archive.org scan amateurworkillus05lond). Metric figures and the tools are ours.

Matériaux

2

Outils requis

4

Blueprints liés

Ces blueprints partagent des connaissances — techniques, matériaux ou principes

CC0 Domaine public

Ce blueprint est publié sous CC0. Vous êtes libre de copier, modifier, distribuer et utiliser ce travail pour tout usage, sans demander la permission.

Soutenez le Maker en achetant des produits via son Blueprint où il perçoit une Commission Maker définie par les Vendeurs, ou créez une nouvelle itération de ce Blueprint et incluez-le comme connexion dans votre propre Blueprint pour partager les revenus.

Commentaires