A paint for putting silver electrodes on ceramic, glass or mica. Silver oxide and a little ceramic flux are held in purified dextrin dissolved in water. The wet paint conducts electricity, so a capacitor can be measured while it is being painted. On firing, the silver oxide turns into a silver film held on by the flux. Dextrin needs no alcohol against foam, and silver nitrate does not attack it while the paint is in use. Source: Robert B. Gray, US 2,695,275 (Erie Resistor, 1954), Example 3. Unknown: how the dextrin is purified. Gray does not give it. Also not given: which flux, and the firing heat. Bismuth subnitrate, one of the fluxes Gray names, is ours. Picture drawn by Youblob.
Débutant
1 day

Consignes

1

Dissolve 4 g purified dextrin in the water

For 100 g of paint: dissolve 4 g purified dextrin in the water. The water is the balance, about 31 to 44 g. Unknown: how the dextrin is purified. Gray does not give it.

Matériaux pour cette étape :

Dextrine purifiéeDextrine purifiée4 g
Eau distilléeEau distillée1 as required

Outils nécessaires :

Balance à fléauBalance à fléau
Bécher en borosilicateBécher en borosilicate
Baguette en verre borosilicatéBaguette en verre borosilicaté
2

Grind in silver oxide and flux

Grind 50 g precipitated silver oxide and 2 to 10 g ceramic flux into the solution until smooth. Gray gives the flux only as a class; ours: bismuth subnitrate, one of the common fluxes he names. The right amount depends on the ceramic it will be fired onto.

Matériaux pour cette étape :

Oxyde d'argentOxyde d'argent50 g
Sous-nitrate de bismuthSous-nitrate de bismuth1 as required

Outils nécessaires :

Balance à fléauBalance à fléau
Mortier et pilonMortier et pilon
Gants en nitrileGants en nitrile
3

Stir in up to 5 g silver nitrate

Stir in 0 to 5 g silver nitrate; it makes the wet paint conduct better. Dextrin is not attacked by it in normal use, and the paint can stand for hours without stirring. Silver nitrate stains and burns skin: gloves.

Matériaux pour cette étape :

Nitrate d'argentNitrate d'argent1 as required

Outils nécessaires :

Balance à fléauBalance à fléau
Baguette en verre borosilicatéBaguette en verre borosilicaté
Gants en nitrileGants en nitrile

Matériaux

5

Outils requis

5

CC0 Domaine public

Ce blueprint est publié sous CC0. Vous êtes libre de copier, modifier, distribuer et utiliser ce travail pour tout usage, sans demander la permission.

Soutenez le Maker en achetant des produits via son Blueprint où il perçoit une Commission Maker définie par les Vendeurs, ou créez une nouvelle itération de ce Blueprint et incluez-le comme connexion dans votre propre Blueprint pour partager les revenus.

Commentaires

(0)

Se connecter pour participer à la discussion

Chargement des commentaires...