Reformate: Straight-Run Naphtha over Platinum-Alumina-Fluorine Catalyst at 874 °F and 500 psi (Haensel, UOP, US 2,479,110)
Charlie

Créé par

Charlie

29. octobre 2026DE
1
0
0
0
0

Reformate: Straight-Run Naphtha over Platinum-Alumina-Fluorine Catalyst at 874 °F and 500 psi (Haensel, UOP, US 2,479,110)

Straight-run naphtha knocks badly in an engine. Passed hot and under pressure over Haensel's platinum catalyst, its molecules are reshaped into aromatics and smaller ones, and the octane number nearly doubles. Result (Ex. I): a Pennsylvania naphtha of octane 41.8 gave 82.5 % by volume of reformate of octane 78.8 (A.S.T.M. motor method). Variable: reforming temperature. At 824 °F: 95.9 % by weight, octane 65.7, too cool. At 874 °F: 83.2 %, octane 78.8; more of the charge goes to gas. Source: Haensel, US 2,479,110 (1949), Ex. I-II. Not given: reactor size, how the products are fractionated. Hot hydrogen and oil vapour under pressure: fire risk. Picture drawn by Youblob.
Expert
1 day

Consignes

1

Pack the catalyst in a fixed bed

Put the platinum reforming catalyst in the reaction zone as a fixed bed. The oil is passed through it, upward or downward.

Outils nécessaires :

Catalyseur de reformage au platineCatalyseur de reformage au platine
Réacteur tubulaire à lit fixeRéacteur tubulaire à lit fixe
2

Feed a straight-run naphtha

Use a straight-run naphtha. Haensel's: a Pennsylvania naphtha boiling from 226 to 350 °F, with an A.S.T.M. motor octane number of 41.8.

Matériaux pour cette étape :

NaphtaNaphta1 as required

Outils nécessaires :

Réservoir à pétroleRéservoir à pétrole
3

Start with hydrogen

The reaction can make enough hydrogen for itself, but the patent prefers to bring hydrogen in from outside at the start and then recycle it, so the reaction zone always holds enough.

Outils nécessaires :

HydrogèneHydrogène
Bouteille de gaz sous pressionBouteille de gaz sous pression
4

Reform at 874 °F, 500 psi

Pass the naphtha over the catalyst at about 874 °F and 500 pounds per square inch, at a weight hourly space velocity of about 2: twice the catalyst's weight in oil each hour.

Outils nécessaires :

Réacteur tubulaire à lit fixeRéacteur tubulaire à lit fixe
Catalyseur de reformage au platineCatalyseur de reformage au platine
ManomètreManomètre
5

Fractionate off the hydrogen, collect the reformate

Fractionate the products to separate the hydrogen, which goes back into the process, and recover the reformate: 82.5 % by volume of the charge, octane 78.8. Ours: a fractionating still.

Outils nécessaires :

Alambic à fractionnerAlambic à fractionner
Bouteille de gaz sous pressionBouteille de gaz sous pression
Réservoir à pétroleRéservoir à pétrole

Matériaux

1
  • 1 as required
    Espace réservé

Outils requis

7

CC0 Domaine public

Ce blueprint est publié sous CC0. Vous êtes libre de copier, modifier, distribuer et utiliser ce travail pour tout usage, sans demander la permission.

Soutenez le Maker en achetant des produits via son Blueprint où il perçoit une Commission Maker définie par les Vendeurs, ou créez une nouvelle itération de ce Blueprint et incluez-le comme connexion dans votre propre Blueprint pour partager les revenus.

Commentaires

(0)

Se connecter pour participer à la discussion

Chargement des commentaires...