Arthur F. Payne · Public domain (1914)
Teaspoon Forged from a Silver Bar (Payne 1914)
A 6-inch silver teaspoon forged out of a small bar of silver, the way a blacksmith forges iron. Arthur Payne called it the hardest of his five spoon methods, but the cheapest, because almost no silver is wasted.
Source: A. F. Payne, Art Metalwork with Inexpensive Equipment (1914), pp. 184–186; annealing from his chapter XI. Cutting the bar from sheet is ours. Picture: Payne's Fig. 158, teaspoons forged this way.
Avancé
1 day
Consignes
1
1
Cut the silver bar
Cut the silver bar
For a teaspoon 6 in long you need a piece of sterling silver 4 in long, ½ in wide and ⅛ in thick. Mark it out and saw it from sheet of that thickness (cutting from sheet is ours).
Matériaux pour cette étape :
Tôle d'argent sterling1 piece 4 × ½ × ⅛ inOutils nécessaires :
Pointe à tracer
Bocfil de bijoutier2
2
Forge out the bowl
Forge out the bowl
Heat the bar until it is almost red-hot, hold it in tongs and forge the bowl out on the anvil. Silver forges more easily when it is nearly red, but never hammer it while it is red-hot: it will crack.
Outils nécessaires :
Bec Bunsen
Pinces
Enclume
Marteau3
3
Work bowl, then shank and handle
Work bowl, then shank and handle
Hammer the bowl until it is hard, then the shank and handle, so the whole spoon is hard before you anneal it again. That saves time.
Outils nécessaires :
Enclume
Marteau4
4
Anneal and repeat
Anneal and repeat
To soften it, heat it to a dull red and plunge it into water, or let it cool. Then go on forging until the spoon is roughly to shape.
Matériaux pour cette étape :
Eau1 as requiredOutils nécessaires :
Bec Bunsen
Pinces
Récipient en verre5
5
Trim with shears and file
Trim with shears and file
Trim the outline with the shears and file the edges smooth.
Outils nécessaires :
Cisailles à métaux renforcées
Limes (lime à main)6
6
Polish out the file marks
Polish out the file marks
Rub out all the scratches and file marks with emery cloth.
Outils nécessaires :
Toile émeri7
7
Anneal to even the fire scale
Anneal to even the fire scale
Anneal the spoon thoroughly once more. Heated silver grows a thin white skin, the fire scale, and this brings it back over the spots where filing and polishing took it off, so the colour is even.
Matériaux pour cette étape :
Eau1 as requiredOutils nécessaires :
Bec Bunsen
Pinces
Récipient en verre8
8
Planish with smooth hammers
Planish with smooth hammers
Planish the spoon on smooth tools with smooth, bright hammers. This makes it stiff again after the annealing.
Outils nécessaires :
Marteau à planer
Enclume
Piquet9
9
Final polish with rouge
Final polish with rouge
Polish it lightly with a soft cotton flannel and a little red rouge.
Outils nécessaires :
Chiffon à polir les bijoux
Rouge à polir de bijoutierMatériaux
2- 1 piece 4 × ½ × ⅛ inEspace réservé
- 2 as requiredEspace réservé
Outils requis
14- Espace réservé
- Espace réservé
- Espace réservé
- Espace réservé
- Espace réservé
- Espace réservé
- Espace réservé
- Espace réservé
- Espace réservé
- Espace réservé
- Espace réservé
- Espace réservé
- Espace réservé
- Espace réservé
Ce plan fabrique
Blueprints liés
Ces blueprints partagent des connaissances — techniques, matériaux ou principes
CC0 Domaine public
Ce blueprint est publié sous CC0. Vous êtes libre de copier, modifier, distribuer et utiliser ce travail pour tout usage, sans demander la permission.
Soutenez le Maker en achetant des produits via son Blueprint où il perçoit une Commission Maker définie par les Vendeurs, ou créez une nouvelle itération de ce Blueprint et incluez-le comme connexion dans votre propre Blueprint pour partager les revenus.