Acrylic Block: Methyl Methacrylate Syrup Cast in Layers between Glass
Charlie

Dibuat oleh

Charlie

20. Oktober 2026DE
5
0
0
0
0

Acrylic Block: Methyl Methacrylate Syrup Cast in Layers between Glass

A thick acrylic block cannot be cast flawless in one pour. Tattersall (ICI, US 2,071,907, 1937) built it up in layers: pour 1/2 inch of syrup on a level glass plate, let it set for a day at room temperature, pour the next 1/2 inch on top, cover with a second glass plate, wait another day, then heat the sandwich at 80 °C. Each 1/2 inch layer shrinks to about 1/3 inch. The glass gives both faces a finished polish with no grinding. The picture: our diagram.
Menengah
3 days

Instruksi

1

Level the bottom plate

Set a glass plate on a ledge in a wooden frame, on a body of plaster of Paris, and level it carefully. The example sheet was 10 by 18 inches.

Alat yang dibutuhkan:

Kaca lembaranKaca lembaran
Bingkai kayuBingkai kayu
Gips (Plaster of Paris)Gips (Plaster of Paris)
Waterpas 1,5 mWaterpas 1,5 m
2

Pour the first 1/2 inch

Pour room-temperature syrup 1/2 inch deep (about 1.5 litres for 10 by 18 inches; our figure). Cover against dust, but do not put the top plate on yet. Leave 24 hours at about 20 °C.

Material untuk langkah ini:

Sirup metil metakrilatSirup metil metakrilat3 l

Alat yang dibutuhkan:

Sarung tangan karetSarung tangan karet
Termometer LaboratoriumTermometer Laboratorium
3

Pour the next layer and cover

Pour a second 1/2 inch layer on the first. Lower the top glass plate onto it so it rests on the syrup and keeps pressing on it. Leave another 24 hours at about 20 °C. For a thicker block repeat the layers, a day apart, and put the plate on the last one.

Alat yang dibutuhkan:

Kaca lembaranKaca lembaran
4

Heat at 80 °C

Take the glass sandwich out of the frame and heat it for three hours at 80 °C to finish the polymerisation.

Alat yang dibutuhkan:

Oven pengeringanOven pengeringan
Termometer LaboratoriumTermometer Laboratorium
Sarung Tangan Tahan PanasSarung Tangan Tahan Panas
5

Spring off the glass

Spring the glass plates off the block with a knife blade. Both faces come out smooth and polished.

Alat yang dibutuhkan:

Pisau KerajinanPisau Kerajinan
Sarung tangan karetSarung tangan karet

Bahan

1

Alat yang Diperlukan

9

Cetak biru ini membuat

Blueprint terkait

Blueprint ini berbagi pengetahuan — teknik, bahan, atau prinsip

CC0 Domain Publik

Cetak biru ini dirilis di bawah CC0. Anda bebas untuk menyalin, memodifikasi, mendistribusikan, dan menggunakan karya ini untuk tujuan apa pun, termasuk komersial, tanpa meminta izin.

Dukung Maker dengan membeli produk melalui Cetak Biru mereka di mana mereka mendapatkan Komisi Pembuat yang ditetapkan oleh Penjual, atau buat iterasi baru dari Cetak Biru ini dan masukkan sebagai koneksi di milik Anda sendiri.