Barium-Calcium Ferrite Disc Magnet: Part of the Barium Replaced by Calcium (Went, Philips 1956, Ex. 21)
Charlie

Dibuat oleh

Charlie

28. Oktober 2026DE
0
0
0
0
0

Barium-Calcium Ferrite Disc Magnet: Part of the Barium Replaced by Calcium (Went, Philips 1956, Ex. 21)

A ceramic magnet in which part of the barium is replaced by calcium: 0.06 mol barium carbonate and 0.04 mol calcium carbonate to 0.6 mol iron oxide, milled, fired in oxygen, milled again, pressed and passed quickly through a hot furnace. Went's rod held 1,660 gauss with a coercive force of 1,210 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 21. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Lanjutan
2 days

Instruksi

1

Weigh barium carbonate, chalk and iron oxide

Weigh 11.84 g barium carbonate (0.06 mol), 4.004 g calcium carbonate (0.04 mol) and 99.55 g ferric oxide (0.6 mol). Barium carbonate is poisonous if swallowed: gloves and a dust respirator.

Material untuk langkah ini:

Barium karbonat (witherit)Barium karbonat (witherit)11.84 g
Kalsium karbonat (kapur tulis halus)Kalsium karbonat (kapur tulis halus)4.004 g
Besi(III) OksidaBesi(III) Oksida99.55 g

Alat yang dibutuhkan:

Neraca lenganNeraca lengan
Sarung tangan karetSarung tangan karet
Respirator P100Respirator P100
2

Mill with alcohol 4 hours and dry

Grind the mixture with alcohol in a ball mill for 4 hours, then dry it.

Alat yang dibutuhkan:

Ball Mill BesiBall Mill Besi
Etanol mutu laboratorium, 95 %Etanol mutu laboratorium, 95 %
Oven pengeringanOven pengeringan
3

Presinter in oxygen at 1000 °C for 2 hours

Fire the dry powder in oxygen at 1000 °C for 2 hours (ours: a tube furnace fed from an oxygen cylinder).

Alat yang dibutuhkan:

Tungku TabungTungku Tabung
OksigenOksigen
Tabung gas bertekananTabung gas bertekanan
Sarung Tangan Tahan PanasSarung Tangan Tahan Panas
4

Mill again 4 hours, dry, press at 1.5 t/cm²

Grind with alcohol in the ball mill for 4 hours, dry, and press at 1.5 tonnes per cm² (ours: discs instead of rods).

Alat yang dibutuhkan:

Ball Mill BesiBall Mill Besi
Etanol mutu laboratorium, 95 %Etanol mutu laboratorium, 95 %
Oven pengeringanOven pengeringan
Mesin pres hidrolikMesin pres hidrolik
Cetakan press cakramCetakan press cakram
5

Pass through a 1200 °C zone in 10 minutes

Sinter at 1200 °C by passing the pieces through a 10 cm hot zone at 10 mm per minute, which is 10 minutes in the heat.

Alat yang dibutuhkan:

Tungku TabungTungku Tabung
Sarung Tangan Tahan PanasSarung Tangan Tahan Panas
6

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

Alat yang dibutuhkan:

ElektromagnetElektromagnet
KompasKompas

Bahan

3

Alat yang Diperlukan

14

Cetak biru ini membuat

Blueprint terkait

Blueprint ini berbagi pengetahuan — teknik, bahan, atau prinsip

CC0 Domain Publik

Cetak biru ini dirilis di bawah CC0. Anda bebas untuk menyalin, memodifikasi, mendistribusikan, dan menggunakan karya ini untuk tujuan apa pun, termasuk komersial, tanpa meminta izin.

Dukung Maker dengan membeli produk melalui Cetak Biru mereka di mana mereka mendapatkan Komisi Pembuat yang ditetapkan oleh Penjual, atau buat iterasi baru dari Cetak Biru ini dan masukkan sebagai koneksi di milik Anda sendiri.

Diskusi

(0)

Masuk untuk bergabung dengan diskusi

Memuat komentar...