Barium Ferrite Disc Magnet: Fired in Carbon Dioxide, Pressed at 12 t/cm² (Went, Philips 1956, Ex. 33)
Charlie

Dibuat oleh

Charlie

28. Oktober 2026DE
0
0
0
0
0

Barium Ferrite Disc Magnet: Fired in Carbon Dioxide, Pressed at 12 t/cm² (Went, Philips 1956, Ex. 33)

A barium ferrite made with more iron oxide, 0.4 mol barium carbonate to 3.6 mol, fired an hour at 1300 °C in carbon dioxide. Little oxygen gives the hexagonal crystal BaFe18O27, with some iron in the lower state. It is milled again, bound with nitrocellulose or polyvinyl alcohol, and pressed hard at 12 tonnes per cm². Went's rod held 1,260 gauss with a coercive force of 700 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 33. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Lanjutan
2 days

Instruksi

1

Weigh barium carbonate and iron oxide

Weigh 79.4 g barium carbonate (0.4 mol) and 580.9 g ferric oxide (3.6 mol). Barium carbonate is poisonous if swallowed: gloves and a dust respirator.

Material untuk langkah ini:

Barium karbonat (witherit)Barium karbonat (witherit)79.4 g
Besi(III) OksidaBesi(III) Oksida580.9 g

Alat yang dibutuhkan:

Neraca lenganNeraca lengan
Sarung tangan karetSarung tangan karet
Respirator P100Respirator P100
2

Mill 15.5 hours, press a pastille, fire in CO2

Grind with alcohol in a ball mill for 15.5 hours, dry, and press into a pastille. Heat it at 1300 °C in carbon dioxide for 1 hour (ours: a tube furnace fed from a CO2 cylinder).

Alat yang dibutuhkan:

Ball Mill BesiBall Mill Besi
Etanol mutu laboratorium, 95 %Etanol mutu laboratorium, 95 %
Oven pengeringanOven pengeringan
Mesin pres hidrolikMesin pres hidrolik
Cetakan press cakramCetakan press cakram
Tungku TabungTungku Tabung
Gas karbon dioksidaGas karbon dioksida
Tabung gas bertekananTabung gas bertekanan
Sarung Tangan Tahan PanasSarung Tangan Tahan Panas
3

Pulverise, mill 14 hours, bind

Crush the cooled pastille and grind it with alcohol for 14 hours. Press the powder into a pastille again with a ceramic binder (ours: polyvinyl alcohol, one of the two named), then crush it to grains.

Material untuk langkah ini:

Bubuk polivinil alkoholBubuk polivinil alkohol1 as required

Alat yang dibutuhkan:

Ball Mill BesiBall Mill Besi
Etanol mutu laboratorium, 95 %Etanol mutu laboratorium, 95 %
Mesin pres hidrolikMesin pres hidrolik
Cetakan press cakramCetakan press cakram
4

Press at 12 tonnes per cm²

Press the grains at 12 tonnes per cm² (ours: discs instead of rods). The patent describes no further firing.

Alat yang dibutuhkan:

Mesin pres hidrolikMesin pres hidrolik
Cetakan press cakramCetakan press cakram
5

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

Alat yang dibutuhkan:

ElektromagnetElektromagnet
KompasKompas

Bahan

3

Alat yang Diperlukan

14

Cetak biru ini membuat

Blueprint terkait

Blueprint ini berbagi pengetahuan — teknik, bahan, atau prinsip

CC0 Domain Publik

Cetak biru ini dirilis di bawah CC0. Anda bebas untuk menyalin, memodifikasi, mendistribusikan, dan menggunakan karya ini untuk tujuan apa pun, termasuk komersial, tanpa meminta izin.