Barium Ferrite Disc Magnet from Natural Magnetite, Presintered at 900 °C (Went, Philips 1956, Ex. 36, Procedure 1)
A barium ferrite magnet made from natural magnetite instead of ferric oxide: barium carbonate and magnetite ground 18 hours, presintered 3 hours at 900 °C, ground again 18 hours, pressed and sintered 2 hours at 1200 °C. Went's rod held 1,450 gauss with a coercive force of 2,425 oersted.
Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 36. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Lanjutan
2 days
Instruksi
1
1
Weigh barium carbonate and magnetite
Weigh barium carbonate and magnetite
Weigh 9.9 g barium carbonate (0.05 mol) and 46.9 g natural magnetite, Fe3O4 (0.20 mol). Barium carbonate is poisonous if swallowed: gloves and a dust respirator.
Material untuk langkah ini:
Barium karbonat (witherit)9.9 g
Magnetit46.9 gAlat yang dibutuhkan:
Neraca lengan
Sarung tangan karet
Respirator P1002
2
Grind 18 hours in a ball mill
Grind 18 hours in a ball mill
Grind the mixture in a ball mill for 18 hours. The patent does not say whether wet or dry.
Alat yang dibutuhkan:
Ball Mill Besi
Respirator P1003
3
Presinter at 900 °C for 3 hours
Presinter at 900 °C for 3 hours
Fire the ground mixture at 900 °C for three hours and let it cool.
Alat yang dibutuhkan:
Tungku Muffle
Krus dengan tutup (porselen)
Penjepit Kowi
Sarung Tangan Tahan Panas4
4
Grind 18 hours in a ball mill
Grind 18 hours in a ball mill
Grind it again in a ball mill for 18 hours. The patent does not say whether wet or dry.
Alat yang dibutuhkan:
Ball Mill Besi
Respirator P1005
5
Press at 1.5 t/cm²
Press at 1.5 t/cm²
Press at 1.5 tonnes per cm² (ours: discs instead of a rod).
Alat yang dibutuhkan:
Mesin pres hidrolik
Cetakan press cakram6
6
Sinter at 1200 °C for 2 hours
Sinter at 1200 °C for 2 hours
Sinter at 1200 °C for 2 hours. The patent gives no atmosphere for this example. Went's rod: 1,450 gauss, 2,425 oersted.
Alat yang dibutuhkan:
Tungku Muffle
Penjepit Kowi
Sarung Tangan Tahan Panas7
7
Magnetise the discs
Magnetise the discs
The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.
Alat yang dibutuhkan:
Elektromagnet
KompasAlat yang Diperlukan
12- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
Cetak biru ini membuat
Blueprint terkait
Blueprint ini berbagi pengetahuan — teknik, bahan, atau prinsip
CC0 Domain Publik
Cetak biru ini dirilis di bawah CC0. Anda bebas untuk menyalin, memodifikasi, mendistribusikan, dan menggunakan karya ini untuk tujuan apa pun, termasuk komersial, tanpa meminta izin.
Dukung Maker dengan membeli produk melalui Cetak Biru mereka di mana mereka mendapatkan Komisi Pembuat yang ditetapkan oleh Penjual, atau buat iterasi baru dari Cetak Biru ini dan masukkan sebagai koneksi di milik Anda sendiri.