Barium Ferrite Disc Magnet from Natural Magnetite, Ground Half an Hour Only (Went, Philips 1956, Ex. 36, Procedure 3)
Charlie

Dibuat oleh

Charlie

28. Oktober 2026DE
2
0
0
0
0

Barium Ferrite Disc Magnet from Natural Magnetite, Ground Half an Hour Only (Went, Philips 1956, Ex. 36, Procedure 3)

A barium ferrite magnet from barium carbonate and natural magnetite, ground for half an hour only, pressed straight away and sintered 4 hours at 1200 °C. Went's rod held 1,345 gauss with a coercive force of 1,215 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 36. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Lanjutan
2 days

Instruksi

1

Weigh barium carbonate and magnetite

Weigh 9.9 g barium carbonate (0.05 mol) and 46.9 g natural magnetite, Fe3O4 (0.20 mol). Barium carbonate is poisonous if swallowed: gloves and a dust respirator.

Material untuk langkah ini:

Barium karbonat (witherit)Barium karbonat (witherit)9.9 g
MagnetitMagnetit46.9 g

Alat yang dibutuhkan:

Neraca lenganNeraca lengan
Sarung tangan karetSarung tangan karet
Respirator P100Respirator P100
2

Grind half an hour in a ball mill

Grind the mixture in a ball mill for half an hour. The patent does not say whether wet or dry.

Alat yang dibutuhkan:

Ball Mill BesiBall Mill Besi
Respirator P100Respirator P100
3

Press at 1.5 t/cm²

Press at 1.5 tonnes per cm² (ours: discs instead of a rod).

Alat yang dibutuhkan:

Mesin pres hidrolikMesin pres hidrolik
Cetakan press cakramCetakan press cakram
4

Sinter at 1200 °C for 4 hours

Sinter at 1200 °C for 4 hours. The patent gives no atmosphere for this example. Went's rod: 1,345 gauss, 1,215 oersted.

Alat yang dibutuhkan:

Tungku MuffleTungku Muffle
Penjepit KowiPenjepit Kowi
Sarung Tangan Tahan PanasSarung Tangan Tahan Panas
5

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

Alat yang dibutuhkan:

ElektromagnetElektromagnet
KompasKompas

Bahan

2

Alat yang Diperlukan

11

Cetak biru ini membuat

Blueprint terkait

Blueprint ini berbagi pengetahuan — teknik, bahan, atau prinsip

CC0 Domain Publik

Cetak biru ini dirilis di bawah CC0. Anda bebas untuk menyalin, memodifikasi, mendistribusikan, dan menggunakan karya ini untuk tujuan apa pun, termasuk komersial, tanpa meminta izin.

Dukung Maker dengan membeli produk melalui Cetak Biru mereka di mana mereka mendapatkan Komisi Pembuat yang ditetapkan oleh Penjual, atau buat iterasi baru dari Cetak Biru ini dan masukkan sebagai koneksi di milik Anda sendiri.

Diskusi

(0)

Masuk untuk bergabung dengan diskusi

Memuat komentar...