Hydroxyl-Ended Silicone Oil: D4 Opened with Potash, Then Water (Ceyzeriat 1964)
Youblob · CC0
Charlie

Dibuat oleh

Charlie

27. Oktober 2026DE
1
0
0
0
0

Hydroxyl-Ended Silicone Oil: D4 Opened with Potash, Then Water (Ceyzeriat 1964)

A trace of hot potash opens the ring of D4 and strings it into a long, thick chain. Water added a little at a time then cuts the chains back and leaves hydroxyl groups on their ends, which is what later lets the oil cure into rubber. This is Louis Ceyzeriat's oil A, the base of every sealant in his patent: 21,000 centistokes, 0.15 % hydroxyl. Source: L. Ceyzeriat (Rhône-Poulenc), US 3,133,891 (1964), column 4. His neutraliser was the precipitated silica Hi-Sil X303; we use our precipitated silica in its place. The potash mix and the equipment are ours. Picture drawn by Youblob.
Lanjutan
2 days

Instruksi

1

Make the 10 % potash

Dissolve 0.5 part of potassium hydroxide in 4.5 parts of water (our arithmetic for 5 parts of a 10 % solution). All parts are by weight.

Material untuk langkah ini:

Kalium hidroksidaKalium hidroksida0.5 parts
AirAir4.5 parts

Alat yang dibutuhkan:

Wadah kacaWadah kaca
Neraca lenganNeraca lengan
2

Heat D4 with the potash under nitrogen

Heat 5000 parts of octamethylcyclotetrasiloxane (it melts at 17.5 °C) with the 5 parts of 10 % potash at 150 °C for 3½ hours under nitrogen. The oil thickens to 31,000 centistokes while hot.

Material untuk langkah ini:

Oktametilsiklotetrasiloksan (D4)Oktametilsiklotetrasiloksan (D4)5000 parts

Alat yang dibutuhkan:

Labu Distilasi KacaLabu Distilasi Kaca
Pelat PemanasPelat Pemanas
TermometerTermometer
PengadukPengaduk
Tabung Gas NitrogenTabung Gas Nitrogen
3

Add water a little at a time

Still hot, add 16.5 parts of water in small portions over 3 hours 40 minutes. The hot oil thins to 1730 centistokes.

Material untuk langkah ini:

AirAir16.5 parts

Alat yang dibutuhkan:

Labu Distilasi KacaLabu Distilasi Kaca
Pelat PemanasPelat Pemanas
TermometerTermometer
PengadukPengaduk
4

Cool, then neutralise with silica

Let it cool for 15 hours. Then stir in 50 parts of precipitated silica to neutralise the potash. The liquid now measures 13,400 centistokes at 25 °C.

Material untuk langkah ini:

Silika endapanSilika endapan50 parts

Alat yang dibutuhkan:

Labu Distilasi KacaLabu Distilasi Kaca
PengadukPengaduk
5

Strip the volatiles at 195–200 °C

Heat it to about 195–200 °C in a current of nitrogen, with a water condenser on the outlet. 655 parts of liquid distil over; 4345 parts of oil A stay in the boiler, 21,000 centistokes at 25 °C with 0.15 % hydroxyl groups.

Alat yang dibutuhkan:

Labu Distilasi KacaLabu Distilasi Kaca
Kumparan kondensorKumparan kondensor
Pelat PemanasPelat Pemanas
TermometerTermometer
Tabung Gas NitrogenTabung Gas Nitrogen
Toples Kaca BertutupToples Kaca Bertutup

Bahan

4

Alat yang Diperlukan

9

CC0 Domain Publik

Cetak biru ini dirilis di bawah CC0. Anda bebas untuk menyalin, memodifikasi, mendistribusikan, dan menggunakan karya ini untuk tujuan apa pun, termasuk komersial, tanpa meminta izin.

Dukung Maker dengan membeli produk melalui Cetak Biru mereka di mana mereka mendapatkan Komisi Pembuat yang ditetapkan oleh Penjual, atau buat iterasi baru dari Cetak Biru ini dan masukkan sebagai koneksi di milik Anda sendiri.

Diskusi

(0)

Masuk untuk bergabung dengan diskusi

Memuat komentar...