Oriented Barium Ferrite Disc Magnet: Binder Dried in a 2400 Oersted Field (Gorter, Philips 1956, Ex. 3)
A ceramic magnet from pre-fired barium ferrite in polyvinyl acetate and acetone, dried in a 2400 oersted field, then pressed, heated and sintered as in Example 2. In the principal direction it held 2,720 gauss with a coercive force of 1,620 oersted and a (BH)max of 1.2 × 10⁶; at right angles 1,610 gauss.
Source: E. W. Gorter, G. W. Rathenau and A. L. Stuyts (Philips), US 2,762,778 (1956), Example 3. They made blocks; disc size is ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Lanjutan
3 days
Instruksi
1
1
Weigh barium carbonate and iron oxide
Weigh barium carbonate and iron oxide
Weigh 450 g barium carbonate and 2000 g ferric oxide. Barium carbonate is poisonous if swallowed: gloves and a dust respirator.
Material untuk langkah ini:
Barium karbonat (witherit)450 g
Besi(III) Oksida2000 gAlat yang dibutuhkan:
Neraca lengan
Sarung tangan karet
Respirator P1002
2
Mill 20 hours under alcohol, dry
Mill 20 hours under alcohol, dry
Grind the mixture in a ball mill under alcohol for 20 hours, then dry it.
Alat yang dibutuhkan:
Ball Mill Besi
Etanol mutu laboratorium, 95 %
Oven pengeringan3
3
Pre-fire: through a 1100 °C zone in 10 minutes
Pre-fire: through a 1100 °C zone in 10 minutes
Pass the dry powder at 20 mm per minute through an electric furnace with a 20 cm hot zone at 1100 °C, in air: 10 minutes in the heat. Let it cool.
Alat yang dibutuhkan:
Tungku Tabung
Krus dengan tutup (porselen)
Sarung Tangan Tahan Panas4
4
Grind 12 hours with alcohol, dry
Grind 12 hours with alcohol, dry
Pulverise the pre-fired material in a ball mill with alcohol for 12 hours, then dry it. This is the pre-fired powder.
Alat yang dibutuhkan:
Ball Mill Besi
Etanol mutu laboratorium, 95 %
Oven pengeringan5
5
Stir into 8 % polyvinyl acetate in acetone
Stir into 8 % polyvinyl acetate in acetone
Dissolve polyvinyl acetate in acetone to a 8 % solution and stir the pre-fired powder into it, 2 cc of solution per gram of powder. The binder burns off later.
Alat yang dibutuhkan:
Polivinil Asetat
Aseton
Neraca lengan6
6
Orient in a 2400 oersted field
Orient in a 2400 oersted field
Put the suspension in a moulding die between the poles of a magnet and apply a first field of 2400 oersted. Remove the binder solution while the field is on.
Alat yang dibutuhkan:
Cetakan press cakram
Elektromagnet
Mesin pres hidrolik7
7
Compress into a block
Compress into a block
Compress the powder into a block as in Example 2. The pressure is not given.
Alat yang dibutuhkan:
Mesin pres hidrolik
Cetakan press cakram8
8
Heat to 500 °C in a 2000 oersted field
Heat to 500 °C in a 2000 oersted field
Put the block in an electric furnace between the magnet's poles. With a second field of 2000 oersted along the first field's direction, heat to 500 °C, which burns off the rest of the binder. Then switch the field off.
Alat yang dibutuhkan:
Tungku Tabung
Elektromagnet
Sarung Tangan Tahan Panas9
9
Sinter: through a 1300 °C zone in 5 minutes
Sinter: through a 1300 °C zone in 5 minutes
Pass the block at 20 mm per minute through an electric furnace in air at 1300 °C with a 10 cm hot zone: about 5 minutes in the heat.
Alat yang dibutuhkan:
Tungku Tabung
Sarung Tangan Tahan Panas10
10
Magnetise in the principal direction
Magnetise in the principal direction
Magnetise the block along the direction of the first field, the principal direction. The patent magnetises it in a field in that direction; ours: an electromagnet. Find the north face with a compass.
Alat yang dibutuhkan:
Elektromagnet
KompasBahan
2- Placeholder
- 2000 gPlaceholder
Alat yang Diperlukan
15- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
Cetak biru ini membuat
Blueprint terkait
Blueprint ini berbagi pengetahuan — teknik, bahan, atau prinsip
CC0 Domain Publik
Cetak biru ini dirilis di bawah CC0. Anda bebas untuk menyalin, memodifikasi, mendistribusikan, dan menggunakan karya ini untuk tujuan apa pun, termasuk komersial, tanpa meminta izin.
Dukung Maker dengan membeli produk melalui Cetak Biru mereka di mana mereka mendapatkan Komisi Pembuat yang ditetapkan oleh Penjual, atau buat iterasi baru dari Cetak Biru ini dan masukkan sebagai koneksi di milik Anda sendiri.