Epoxy Resin

Pierre Castan, a Swiss chemist at the dental firm De Trey Frères, was looking for a resin for dentures. He reacted a phenol carrying two hydroxy groups with epichlorohydrin, then hardened the product with an acid anhydride, and got a hard, clear, unusually adherent solid. Ciba licensed it and sold it as Araldite; in the US Sylvan Greenlee developed epoxies independently. **US 2,324,483**, "Process of preparing synthetic resins", Castan, granted 20. July 1943, claims condensing "a polybasic carboxylic acid anhydride" with the product of "a phenol having at least two phenolic hydroxy groups and of an epichlorhydrine". It does not single out bisphenol A, the phenol most epoxies use today. **Epichlorohydrin is a carcinogen; you start from a two-part kit.** You glue pine lap joints at the right ratio and four wrong ones, then test hardness and break the joints.
शुरुआती
2 hours plus 24 h cure

निर्देश

1

Cut the joint pieces

Saw ten pine strips 100 x 25 mm. Sand one face of each end with 120 grit and dust off. Label five pairs 1:1, 1.25:1, 1:1.25, 1.5:1 and 1:1.5.

इस चरण के लिए सामग्री:

चीड़ का पटराचीड़ का पटरा1 टुकड़ा
रेगमालरेगमाल1 शीट
मास्किंग टेपमास्किंग टेप1 रोल

आवश्यक उपकरण:

हस्त आरीहस्त आरी
इस्पात का पैमानाइस्पात का पैमाना
पेंसिलपेंसिल
2

Measure by syringe

Gloves on. For each ratio draw resin and hardener in separate syringes (1:1 = 2 ml + 2 ml; 1.25:1 = 2.5 + 2; and so on) into its own cup. This assumes a 1:1-by-volume kit - scale to your label.

इस चरण के लिए सामग्री:

दो घटक वाली इपॉक्सीदो घटक वाली इपॉक्सी25 मिली

आवश्यक उपकरण:

नाइट्राइल दस्तानेनाइट्राइल दस्ताने
सिरिंज सेटसिरिंज सेट
अंशांकित मिलाने के प्यालेअंशांकित मिलाने के प्याले
पारदर्शी सुरक्षा चश्मापारदर्शी सुरक्षा चश्मा
3

Mix thoroughly

Stir each cup 2 minutes, scraping the walls and bottom. Unmixed streaks behave like a wrong ratio.

आवश्यक उपकरण:

हिलाने वाली छड़हिलाने वाली छड़
4

Glue and pour

Spread each mix on the sanded ends of its pair, overlap them 25 mm and spring-clamp over wax paper. Pour the rest as a coin-sized puddle on wax paper beside it.

इस चरण के लिए सामग्री:

मोमित काग़ज़मोमित काग़ज़1 शीट

आवश्यक उपकरण:

स्प्रिंग क्लैंपस्प्रिंग क्लैंप
5

Cure 24 hours

Leave everything at room temperature, 20 °C or warmer, for 24 hours. Cold slows the cure.
6

Pencil hardness

Sharpen pencils 6B to 6H and flatten the tips on 400 grit. Push each at 45° across a puddle, from hard down, until one no longer scratches. Record that grade.

आवश्यक उपकरण:

ग्रेफ़ाइट पेंसिल सेटग्रेफ़ाइट पेंसिल सेट
आवर्धक लूपआवर्धक लूप
7

Break the joints

Clamp one strip of a joint in the vise and tap the free end sideways with the mallet until it breaks. Estimate how much of the bond face is torn wood.

आवश्यक उपकरण:

बेंच शिकंजाबेंच शिकंजा
रबर का हथौड़ारबर का हथौड़ा
पारदर्शी सुरक्षा चश्मापारदर्शी सुरक्षा चश्मा
8

Ratio, leftovers, results

Jupyter नोटबुक लोड हो रही है…
9

History & Context

**What the patent specifies:** a resin from a two-hydroxy phenol and epichlorohydrin, hardened by a polybasic acid anhydride. **Modern build (derived):** a two-part kit, most with an amine hardener that cures at room temperature. Epoxy became the glue that holds metal, the matrix of fibreglass and carbon-fibre parts, and the boat-builder's resin. Its limits: it yellows in sunlight, softens with heat, and uncured resin and hardener sensitise skin - which is why the gloves stay on every time.

सामग्री

5

आवश्यक उपकरण

13

CC0 पब्लिक डोमेन

यह ब्लूप्रिंट CC0 के तहत जारी किया गया है। आप बिना अनुमति माँगे इस कार्य को किसी भी उद्देश्य के लिए कॉपी, संशोधित, वितरित और उपयोग करने के लिए स्वतंत्र हैं।

उनके ब्लूप्रिंट के माध्यम से उत्पाद खरीदकर मेकर का समर्थन करें जहाँ वे मेकर कमीशन कमाते हैं जो विक्रेताओं द्वारा निर्धारित होता है, या इस ब्लूप्रिंट का नया संस्करण बनाएँ और राजस्व साझा करने के लिए इसे अपने ब्लूप्रिंट में कनेक्शन के रूप में शामिल करें।

चर्चा

(0)

लॉग इन करें चर्चा में शामिल होने के लिए

टिप्पणियाँ लोड हो रही हैं...