Polypropylene Felt: a Spunbonded Web, Kinney 1967
A polypropylene felt made without weaving or needling: hot filaments are spun, pulled down by an air jet, given an electric charge so they spread apart, and laid in loops on a moving table until they form an even sheet. Kinney's patent (Du Pont, US 3,338,992, 1967) gives every setting for polypropylene. The corona runs at 20 to 25 kV: keep clear of it while it is live.
The picture: the patent's own Fig. 1 (the process) and Fig. 7 (the web).
उन्नत
1 day
निर्देश
1
1
Melt and spin
Melt and spin
Melt polypropylene of melt index 10 in a screw extruder, no hotter than 290 °C. Meter it at 12 g a minute through a 1/4 in. sand filter and a 20-hole spinneret (holes 0.015 in. across): pack block 275 °C, spinneret 260 °C.
इस चरण के लिए सामग्री:
पॉलीप्रोपिलीन की गोलियाँ500 ग्राआवश्यक उपकरण:
प्लास्टिक एक्सट्रूडर
स्पिनरेट
पाइरोमीटर
तराजू
चमड़े के दस्ताने2
2
Quench
Quench
Cool the bundle of filaments in a 6 in. quench chimney blowing 40 cubic feet a minute of room air in from the side.
आवश्यक उपकरण:
वायु संपीडक3
3
Draw with the air jet
Draw with the air jet
Lead the bundle 72 in. down into an air draw jet run at 25 psi: it pulls the filaments with about 3 g of tension and stretches them.
आवश्यक उपकरण:
वायु-खिंचाव जेट
वायु संपीडक
दाबमापी4
4
Charge the filaments
Charge the filaments
8 in. above the jet, let the filaments brush a 1 1/4 in. bar turning at 10 rpm, with a four-point corona 5/8 in. from it at minus 20 to 25 kV (100 to 150 µA). The charge pushes them apart. Keep clear while it is live.
आवश्यक उपकरण:
कोरोना चार्जिंग इकाई5
5
Lay the web
Lay the web
Catch the filaments on a grounded 47 in. square table that moves 26 in. a minute one way and 570 in. a minute the other. Each layer weighs 0.5 oz per square yard; lay several for each sheet.
आवश्यक उपकरण:
बिछाव मेज़6
6
What you get
What you get
An even sheet of fine filaments, about 2.5 denier each, tenacity 2.0 g per denier, stretching 300 % before they break.
आवश्यक उपकरण:
तराजूसामग्री
1- 500 ग्राप्लेसहोल्डर
आवश्यक उपकरण
10- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- 1 vendor sell this, none ship to you yetप्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
यह ब्लूप्रिंट बनाता है
CC0 पब्लिक डोमेन
यह ब्लूप्रिंट CC0 के तहत जारी किया गया है। आप बिना अनुमति माँगे इस कार्य को किसी भी उद्देश्य के लिए कॉपी, संशोधित, वितरित और उपयोग करने के लिए स्वतंत्र हैं।
उनके ब्लूप्रिंट के माध्यम से उत्पाद खरीदकर मेकर का समर्थन करें जहाँ वे मेकर कमीशन कमाते हैं जो विक्रेताओं द्वारा निर्धारित होता है, या इस ब्लूप्रिंट का नया संस्करण बनाएँ और राजस्व साझा करने के लिए इसे अपने ब्लूप्रिंट में कनेक्शन के रूप में शामिल करें।