Casting a Bronze Socketed Spearhead — Bivalve Mould Method
Forge

ایجاد شده توسط

Forge

26. مه 2026NO
۱۲
۰
۰
۱
۰

Casting a Bronze Socketed Spearhead — Bivalve Mould Method

The socketed spearhead was a major advance over the flat tanged point — the hollow socket allowed the shaft to be inserted directly into the head, creating a stronger and more aerodynamic weapon. This design appeared across the Bronze Age world from approximately 2000 BCE and remained in use for over a thousand years.

Creating the socket requires a bivalve mould with a clay core inserted between the two stone halves. The core occupies the space where the socket will be, so when the bronze solidifies around it and the core is broken out, a hollow tube remains. This is one of the earliest examples of core-casting — a technique that later evolved into the lost-wax process for complex hollow sculptures.

The leaf-shaped blade is cast with a raised midrib for rigidity, then the edges are cold-hammered and ground sharp. Two small holes at the socket base allow a pin or binding to lock the shaft in place.

پیشرفته
3-4 hours (casting, core removal, and finishing)

دستورالعمل‌ها

1

Prepare the bivalve mould

Use a two-part soapstone mould with a leaf-shaped spearhead cavity carved into both halves. The cavity should include a raised ridge down the centre of each half — when assembled, these form the midrib channel. Ensure the alignment pegs seat correctly and both halves close without gaps. Coat the cavity surfaces with soot from a smoky fire.

مواد مورد نیاز این مرحله:

Soapstone Block (Steatite)Soapstone Block (Steatite)2 piece
2

Form the clay core for the socket

Mix refractory clay with fine sand to make a stiff paste. Shape it into a tapered cylinder matching the socket cavity — typically 8-10 cm long and 2-2.5 cm in diameter, tapering to a blunt point. Let the core dry thoroughly for at least one day, then fire it gently near a flame to drive out all moisture. A wet core in contact with molten bronze explodes.

مواد مورد نیاز این مرحله:

Refractory ClayRefractory Clay200 g
Fine SandFine Sand100 g
3

Assemble the mould with core

Place the fired clay core into the socket cavity of one mould half, resting it against the small clay chaplets (support pegs) that keep it centred. Close the second half over it, engaging the alignment pegs. Bind the two halves tightly with wet rawhide strips. Stand the mould upright with the pour funnel at the top and the blade cavity pointing downward.

مواد مورد نیاز این مرحله:

Rawhide StripsRawhide Strips1 m
4

Pre-heat the assembled mould

Place the bound mould near the fire for 30 minutes, rotating occasionally. Both the stone and the clay core must be hot before pouring. The temperature difference between cold stone and 1,050 °C bronze causes the metal to freeze before filling thin sections like the blade edges.
5

Melt and pour the bronze

Melt 400 g of bronze (360 g copper, 40 g tin) in a pre-heated clay crucible. When the metal is fluid and glowing bright orange, lift the crucible with tongs and pour into the mould funnel in one continuous stream. Bronze flows around the clay core and into the blade cavity. Continue pouring until metal appears at the vent holes, confirming the mould is full.

مواد مورد نیاز این مرحله:

CharcoalCharcoal4 kg

ابزارهای مورد نیاز:

Crucible Tongs (long-handled)Crucible Tongs (long-handled)
6

Cool and separate the mould halves

Allow the mould to cool for 15-20 minutes. Cut the rawhide bindings, separate the mould halves, and extract the casting. The spearhead emerges with the clay core still inside the socket, the sprue still attached at the pour channel, and thin flash lines along the mould parting line.
7

Remove the clay core

Break the clay core out of the socket using a pointed bone tool or antler tine. Chip away in small pieces, working from the open end inward. The fired clay should crumble relatively easily. Clean out all core fragments — any remaining clay prevents the shaft from seating fully.

ابزارهای مورد نیاز:

Antler TineAntler Tine
8

Remove sprue and grind the parting line

Score and snap off the sprue. Grind away flash along both sides of the blade where the mould halves met, using a sandstone slab with water. The parting line must be completely smooth — any ridge catches in a wound and weakens the penetration.

مواد مورد نیاز این مرحله:

Sandstone (Abrasive)Sandstone (Abrasive)1 piece
9

Cold-hammer and sharpen the blade edges

Hammer both blade edges on a flat stone anvil to work-harden the bronze. Strike with controlled overlapping blows, working from the midrib outward toward the edge. This compresses the grain structure and dramatically increases hardness. Finish by grinding on a whetstone to a razor-sharp edge along the full length of the blade.

مواد مورد نیاز این مرحله:

WhetstoneWhetstone1 piece

ابزارهای مورد نیاز:

HammerstoneHammerstone
Flat Stone SlabFlat Stone Slab
10

Drill the rivet holes and haft

Using a small flint drill bit rotated between the palms or in a bow drill, bore two small holes through the socket wall near the base — one on each side. Shape a straight ash or hazel shaft to fit snugly in the socket. Insert the shaft, then drive bronze or bone pins through the holes and through the shaft to lock it in place. The spearhead is complete.

مواد

7

ابزارهای لازم

4

مواد نقشه‌های متصل

نقشه‌های مرتبط

این نقشه‌ها دانش مشترکی دارند — تکنیک‌ها، مواد یا اصول

CC0 مالکیت عمومی

این نقشه تحت مجوز CC0 منتشر شده است. شما آزاد هستید آن را کپی، ویرایش، توزیع و برای هر هدفی بدون نیاز به اجازه استفاده کنید.

با خرید محصولات از طریق نقشه از سازنده حمایت کنید و او کمیسیون سازنده تعیین شده توسط فروشندگان، دریافت می‌کند یا یک نسخه جدید از این نقشه ایجاد کنید و آن را به عنوان اتصال در نقشه خود قرار دهید تا درآمد به اشتراک گذاشته شود.

بحث و گفتگو

(0)

ورود برای شرکت در بحث

در حال بارگذاری نظرات...