Forged Ball-Peen Hammer

A 2-pound ball-peen hammer forged from 1½-inch square tool steel; a 6½-inch bar gives two heads. The eye is punched and drifted, the body fullered and rounded so it tapers both ways from a thick centre, then the face is drawn out and swaged and the ball peen rounded in a bottom swage. Both ends are hardened by dipping them in turn, with water dripping on the face, and tempered from the heat held around the eye: dark brown for the face, brown or purple for the peen. The eye cools last, which keeps it tough.
Lengra kominn
4–6 hours

Leiðbeiningar

1

Mark and flatten

Mark the bar with a chisel and centre punch. Flatten the end before punching, or the hole grows too large.

Efni fyrir þetta skref:

Ferstrent verkfærastálFerstrent verkfærastál1 stykki

Nauðsynleg verkfæri:

KörnunardorgKörnunardorg
HeitmeitillHeitmeitill
SmiðjueldstæðiSmiðjueldstæði
SteðjiSteðji
SleggjaSleggja
JárnsmiðstöngJárnsmiðstöng
2

Punch and drift the eye

Punch the eye at the centre-punch mark, drive in a drift and hammer the bulged sides straight.

Nauðsynleg verkfæri:

HeitgatajárnHeitgatajárn
GatvíkkariGatvíkkari
SmíðahamarSmíðahamar
3

Shape the body

Rough out the shape with top and bottom fullers, then round the body at the anvil's rounded edge with a top fuller and set hammer, thicker at the centre than at the ends.

Nauðsynleg verkfæri:

Fuller (rásarjárn)Fuller (rásarjárn)
SetthamarSetthamar
4

Face and peen

Cut the head from the bar from four sides for a square end. Draw out the face, swage it and trim it with a hot chisel; then cut the peen to length, cut off its corners and round it in a bottom swage. Drive the drift through from both sides to taper the eye.

Nauðsynleg verkfæri:

HeitmeitillHeitmeitill
Neðri mótsteðji (neðra mót)Neðri mótsteðji (neðra mót)
GatvíkkariGatvíkkari
5

Grind

Grind both ends, rounding the edges of the face slightly so it does not mark hot work.

Nauðsynleg verkfæri:

BekkslípivélBekkslípivél
6

Harden and temper

Heat the whole head slowly to the hardening heat and hold it by a tong jaw in the eye. Lower about 1½ inches of the face into water, then harden the peen the same way while water drips on the face, keeping the eye hot. Polish the ends; take the face to dark brown and the peen to brown or purple, then dip the ends alternately so the eye cools slowly.

Nauðsynleg verkfæri:

SmiðjueldstæðiSmiðjueldstæði
HerslufataHerslufata
JárnsmiðstöngJárnsmiðstöng
SmergildúkurSmergildúkur
7

Handle

Shave the handle stock to fit the eye tightly, drive the head on, saw a kerf in the handle's top and drive a glued hardwood wedge into it. Trim flush and oil the handle.

Efni fyrir þetta skref:

Harðviðarefni í sköftHarðviðarefni í sköft1 stykki
HarðviðarkíllHarðviðarkíll1 stykki
LínolíaLínolía10 ml

Nauðsynleg verkfæri:

BugtarhefillBugtarhefill
Þversög fyrir tvoÞversög fyrir tvo
SkrúfstykkiSkrúfstykki

Efni

4

Nauðsynleg verkfæri

18

Þessi teikning býr til

CC0 opinbert ríki

Þessi teikning er gefin út undir CC0. Þér er frjálst að afrita, breyta, dreifa og nota þetta verk í hvaða tilgangi sem er, án þess að biðja um leyfi.