Forged Cross-Peen Hammer
Smiths make their own hammers. A bar of high-carbon steel is punched through hot for the eye, the eye is opened to shape with a drift, one end is drawn into a peen, and the head is cut off the bar. It is hardened all over, then tempered by heat run from the middle: the eye and cheeks are left soft (blue) so they do not crack, the faces harder (straw) so they do not dent. The handle is riven ash or hickory, wedged into the eye.
Lengra kominn
A day
Leiðbeiningar
1
1
Square the bar
Square the bar
Forge crucible steel into a square bar about 30 mm across, long enough to hold by one end.
Efni fyrir þetta skref:
Deiglustál2 kg
Viðarkol15 kgNauðsynleg verkfæri:
Smiðjueldstæði
Steðji
Sleggja
Járnsmiðstöng
Leðursvunta
Suðuhanskar
Öryggisgleraugu
Heyrnarhlífar2
2
Punch the eye
Punch the eye
At a yellow heat, drive the hot punch halfway in from one side, turn the bar over and punch through from the other side over the anvil's hole. Cool the punch often.
Efni fyrir þetta skref:
Vatn5 lítrarNauðsynleg verkfæri:
Heitgatajárn
Sleggja
Steðji
Herslufata3
3
Drift the eye
Drift the eye
Drive the drift through the hot eye from both sides to open it to the handle's shape.
Nauðsynleg verkfæri:
Gatvíkkari
Sleggja4
4
Draw the peen
Draw the peen
Mark the head's length. Draw one side of the eye into a wedge-shaped peen with the fuller and flatter, its edge across the handle's line.
Nauðsynleg verkfæri:
Fuller (rásarjárn)
Sléttari
Sleggja5
5
Cut off and dress
Cut off and dress
Cut the head off the bar on the hot-cut hardy. Square and slightly dome the face; round the peen's edge.
Nauðsynleg verkfæri:
Steðjameitill
Sleggja
Þjalasett6
6
Normalise
Normalise
Heat it to a red heat and let it cool in still air, three times, to relieve the forging.
Nauðsynleg verkfæri:
Smiðjueldstæði
Járnsmiðstöng7
7
Harden
Harden
Heat evenly until a magnet no longer sticks, and quench it in warm oil in a lidded bucket, moving it, for a few minutes.
Efni fyrir þetta skref:
Repjuolía5 lítrarNauðsynleg verkfæri:
Smiðjueldstæði
Segull
Málmfata með loki
Járnsmiðstöng
Suðuhanskar8
8
Temper from the eye
Temper from the eye
Sand the faces bright. Heat the middle of the head with the torch and watch the colours run out toward the ends: when the faces reach straw and the eye is blue, quench it in water.
Nauðsynleg verkfæri:
Sandpappírsörk
Própanbrennari
Herslufata
Járnsmiðstöng9
9
Handle
Handle
Shave the handle stock to fit the eye tightly, drive the head on, saw a kerf in the handle's top and drive a glued hardwood wedge into it. Trim flush and oil the handle.
Efni fyrir þetta skref:
Harðviðarefni í sköft1 stykki
Harðviðarkíll1 stykki
Línolía10 mlNauðsynleg verkfæri:
Bugtarhefill
Þversög fyrir tvo
Skrúfstykki10
10
Troubleshooting
Troubleshooting
Hammer making troubleshooting.
Flow
Loading...
Efni
7- 2 kgStaðgengill
- 15 kgStaðgengill
- 5 lítrarStaðgengill
- 5 lítrarStaðgengill
- 1 stykkiStaðgengill
- 1 stykkiStaðgengill
- 10 mlStaðgengill
Nauðsynleg verkfæri
22- Staðgengill
- Staðgengill
- Staðgengill
- Staðgengill
- Staðgengill
- Staðgengill
- Staðgengill
- Staðgengill
- Staðgengill
- Staðgengill
- Staðgengill
- Staðgengill
- Staðgengill
- Staðgengill
- Staðgengill
- Staðgengill
- Staðgengill
- Staðgengill
- Staðgengill
- Staðgengill
- Staðgengill
- Staðgengill
Þessi teikning býr til
Tengd Blueprint
Þessi blueprint deila þekkingu — tækni, efni eða meginreglur
CC0 opinbert ríki
Þessi teikning er gefin út undir CC0. Þér er frjálst að afrita, breyta, dreifa og nota þetta verk í hvaða tilgangi sem er, án þess að biðja um leyfi.
Studdu smiðinn með því að kaupa vörur í gegnum teikningu hans þar sem hann fær þóknun smiða sem seljendur ákvarða, eða búðu til nýja endurskoðun á þessari teikningu og tengdu hana sem tengingu í þinni eigin teikningu til að deila tekjum.