Steel Files: Forged, Cut and Hardened

A file is a bar of high-carbon steel, about 1.0–1.25 % carbon, covered in rows of tiny chisel cuts. The blank is forged with a tang, annealed soft, ground flat, and the teeth are raised one by one with a chisel and hammer: each blow cuts a groove and lifts its edge into a tooth. A single-cut file has one row of parallel cuts, at 65–85° to the length; a double-cut file has a second row crossing the first, for general work the first at 40–45° and the second at 70–80°. The file is then hardened as hard as it will go by quenching it in cold brine, and is never tempered; only the tang is softened so it will not snap. Factories do the same steps by machine.
Lengra kominn
2 days (annealing overnight)

Leiðbeiningar

1

Forge the blank

At a yellow heat, draw the high-carbon steel to the file's section and forge a narrow, pointed tang at one end.

Efni fyrir þetta skref:

HákolefnisstálbitiHákolefnisstálbiti0.5 kg

Nauðsynleg verkfæri:

SmiðjueldstæðiSmiðjueldstæði
SteðjiSteðji
SmíðahamarSmíðahamar
SmiðjutöngSmiðjutöng
2

Anneal

Heat the blank no hotter than a blood-red and let it cool very slowly, shut away from the air; factories leave blanks in closed boxes in the furnace for 24–36 hours. Cooled in open air it would harden again.

Nauðsynleg verkfæri:

SmiðjueldstæðiSmiðjueldstæði
3

Straighten and grind

Straighten the blank, grind off the scale and make the faces flat and even, or the teeth will not be uniform.

Nauðsynleg verkfæri:

BrýnsluhjólBrýnsluhjól
4

Cut the teeth

Hold the chisel at an angle and strike it, then move it a small, regular distance and strike again; each blow raises one tooth. For a double cut, cut the first row (overcut), then a second row crossing it (upcut). To cut the other face, turn the file over on a pewter plate so the finished teeth are not crushed.

Nauðsynleg verkfæri:

ÞjalarhöggmeitillÞjalarhöggmeitill
SmíðahamarSmíðahamar
SteðjiSteðji
Tinplata (pjátur)Tinplata (pjátur)
5

Harden

Heat the file evenly to its hardening heat and plunge it into a bath of cold brine, which cools faster than water and leaves it harder. Do not temper it.

Efni fyrir þetta skref:

SaltSalt1 kg

Nauðsynleg verkfæri:

SmiðjueldstæðiSmiðjueldstæði
FataFata
SmiðjutöngSmiðjutöng
6

Soften the tang

Reheat the tang alone so it is no longer glass-hard: a fully hard tang snaps when the handle is driven on. Clean and oil the file.

Nauðsynleg verkfæri:

SmiðjueldstæðiSmiðjueldstæði
SmiðjutöngSmiðjutöng

Efni

2

Nauðsynleg verkfæri

8

CC0 opinbert ríki

Þessi teikning er gefin út undir CC0. Þér er frjálst að afrita, breyta, dreifa og nota þetta verk í hvaða tilgangi sem er, án þess að biðja um leyfi.

Studdu smiðinn með því að kaupa vörur í gegnum teikningu hans þar sem hann fær þóknun smiða sem seljendur ákvarða, eða búðu til nýja endurskoðun á þessari teikningu og tengdu hana sem tengingu í þinni eigin teikningu til að deila tekjum.

Umræða

(0)

Skrá inn til að taka þátt í umræðunni

Hleður athugasemdum...