Jewellers' Rouge Precipitated from Copperas, Ure 1839
Rouge is fine red iron oxide, the last polish for metal and lenses. Ure (1839) gives the best polishing powder: add soda solution to copperas solution, wash and dry the precipitate, and heat it gently in shallow vessels until it turns a deep brown red. Grind and wash it fine, and bind some in wax and tallow as a bar.
The picture: iron(III) oxide powder.
Miðlungs
Two days
Leiðbeiningar
1
1
Two solutions
Two solutions
Dissolve the copperas in warm water in one jar and the washing soda in water in a bucket. Weigh both.
Efni fyrir þetta skref:
Járnsúlfat250 g
Vatn3 lítrarNauðsynleg verkfæri:
Þvottasódi
Skálavog
Glerkrukka
Fata
Gúmmíhanskar2
2
Precipitate
Precipitate
Pour the soda solution into the copperas solution slowly, stirring, until no more solid forms. Let the solid settle.
Nauðsynleg verkfæri:
Fata
Hræriár úr tré
Gúmmíhanskar3
3
Wash
Wash
Pour off the clear liquid, fill with fresh water, stir and let it settle again. Repeat several times, then drain the solid on filter paper.
Efni fyrir þetta skref:
Vatn10 lítrarNauðsynleg verkfæri:
Fata
Glertrekt með stút
Síupappír4
4
Calcine gently
Calcine gently
Dry the solid in a shallow dish on the sand bath, then keep heating it gently, stirring now and then, until it is all a deep brown red.
Nauðsynleg verkfæri:
Uppgufunarskál
Sandbað5
5
Grind and wash fine
Grind and wash fine
Grind it in the mortar, stir it into water, wait a minute and pour the cloudy water off the coarse grains into another jar. Let that settle, pour off the water and dry the fine powder. This is the rouge.
Efni fyrir þetta skref:
Vatn2 lítrarNauðsynleg verkfæri:
Mortél og mortélstautur
Glerkrukka
Uppgufunarskál
Sandbað6
6
A rouge bar
A rouge bar
Melt tallow and beeswax together, stir in rouge until it is a stiff paste, and pour it into a small pan to set. Rub the bar on a felt or cloth buff to polish.
Efni fyrir þetta skref:
Tólg40 g
Býflugnavax20 gNauðsynleg verkfæri:
Vatnsbaðspottur
Grunn málmpanna
Ullarþóf7
7
How much rouge
How much rouge
Hleð Jupyter-vinnubók…
Efni
4- 250 gStaðgengill
- 15 lítrarStaðgengill
- 40 gStaðgengill
- 20 gStaðgengill
Nauðsynleg verkfæri
14- Staðgengill
- Staðgengill
- Staðgengill
- Staðgengill
- Staðgengill
- Staðgengill
- Staðgengill
- Staðgengill
- Staðgengill
- Staðgengill
- Staðgengill
- Staðgengill
- Staðgengill
- Staðgengill
Þessi teikning býr til
Tengd Blueprint
Þessi blueprint deila þekkingu — tækni, efni eða meginreglur
CC0 opinbert ríki
Þessi teikning er gefin út undir CC0. Þér er frjálst að afrita, breyta, dreifa og nota þetta verk í hvaða tilgangi sem er, án þess að biðja um leyfi.
Studdu smiðinn með því að kaupa vörur í gegnum teikningu hans þar sem hann fær þóknun smiða sem seljendur ákvarða, eða búðu til nýja endurskoðun á þessari teikningu og tengdu hana sem tengingu í þinni eigin teikningu til að deila tekjum.