Lactide is the ring-shaped double molecule of lactic acid, the monomer from which PLA is made. Schneider's du Pont patent (US 2,703,316, 1955) drives the water out of lactic acid, condenses it under vacuum to a syrupy low polymer, then heats that to 200–250 °C at 8–10 mm so that lactide distils off. For a tough plastic it must be very pure: recrystallise it from ethyl acetate until it melts at 120 °C or higher (best 123–125 °C). The picture: our diagram.
Lengra kominn
1–2 days

Leiðbeiningar

1

Drive off the water

Distil the lactic acid at atmospheric pressure at 120–130 °C until nearly all the water of dilution has gone.

Efni fyrir þetta skref:

Mjólkursýra (tæknileg)Mjólkursýra (tæknileg)1 stykki

Nauðsynleg verkfæri:

KúlukolbaKúlukolba
EimsvalaspírallEimsvalaspírall
HitaplataHitaplata
OlíubaðOlíubað
RannsóknastofuhitamælirRannsóknastofuhitamælir
2

Condense under vacuum

Continue distilling under 17–35 mm of mercury. Water of esterification comes off and the acid becomes a syrupy low polymer (polylactic acid).

Nauðsynleg verkfæri:

LofttæmidælaLofttæmidæla
LofttæmismælirLofttæmismælir
KuldagildraKuldagildra
OlíubaðOlíubað
RannsóknastofuhitamælirRannsóknastofuhitamælir
3

Crack to lactide

Lower the pressure to 8–10 mm and raise the temperature to 200–250 °C. Lactide distils at 130–140 °C (10–13 mm) and sets to a soft crystalline solid.

Nauðsynleg verkfæri:

LofttæmidælaLofttæmidæla
LofttæmismælirLofttæmismælir
EimsvalaspírallEimsvalaspírall
OlíubaðOlíubað
RannsóknastofuhitamælirRannsóknastofuhitamælir
Hitaþolnir hanskarHitaþolnir hanskar
4

Recrystallise from ethyl acetate

Recrystallise the crude lactide from ethyl acetate, filter and dry. Repeat: in the patent the melting point rose from 114–115 °C after the first crystallisation to 118, 123–124 and 124–125 °C after the fourth.

Nauðsynleg verkfæri:

EtýlasetatEtýlasetat
Hitaþolinn glerbikarHitaþolinn glerbikar
HitaplataHitaplata
Büchner-trekt (postulín)Büchner-trekt (postulín)
SíupappírSíupappír
Hlífðargleraugu gegn efnaslettumHlífðargleraugu gegn efnaslettum
5

Check the melting point

Put a few crystals in a capillary tube and warm slowly. Lactide melting at 120 °C or above is fit for making PLA; below 120 °C it gives a brittle polymer.

Nauðsynleg verkfæri:

Hárpípa úr gleriHárpípa úr gleri
RannsóknastofuhitamælirRannsóknastofuhitamælir
OlíubaðOlíubað

Efni

1

Nauðsynleg verkfæri

15

Þessi teikning býr til

CC0 opinbert ríki

Þessi teikning er gefin út undir CC0. Þér er frjálst að afrita, breyta, dreifa og nota þetta verk í hvaða tilgangi sem er, án þess að biðja um leyfi.

Studdu smiðinn með því að kaupa vörur í gegnum teikningu hans þar sem hann fær þóknun smiða sem seljendur ákvarða, eða búðu til nýja endurskoðun á þessari teikningu og tengdu hana sem tengingu í þinni eigin teikningu til að deila tekjum.

Umræða

(0)

Skrá inn til að taka þátt í umræðunni

Hleður athugasemdum...