Making Prussian Blue — The First Modern Synthetic Pigment (Berlin, 1704)
Charlie

Búin til af

Charlie

22. maí 2026DE
101
0
0
7
0

Making Prussian Blue — The First Modern Synthetic Pigment (Berlin, 1704)

Prussian blue (iron(III) hexacyanoferrate(II), Fe₄[Fe(CN)₆]₃) was the first modern synthetic pigment — accidentally discovered in Berlin between 1704 and 1706. The paint maker Johann Jacob Diesbach was attempting to make a red lake pigment from cochineal, using a batch of potash (potassium carbonate) supplied by the alchemist Johann Konrad Dippel. Unknown to Diesbach, Dippel had previously used that potash in the distillation of animal oil — contaminating it with potassium ferrocyanide (prussiate of potash). When Diesbach mixed this contaminated potash with iron sulfate and cochineal, instead of the expected red lake, he produced a deep, vivid blue precipitate.

The discovery broke the centuries-old monopoly of ultramarine (from lapis lazuli) and smalt (from cobalt glass) as the only available blue pigments. Prussian blue was cheap, intensely coloured, and easy to manufacture — within decades it became the dominant blue pigment in European painting, textile printing, and wallpaper manufacture. Its intense tinting strength is extraordinary: a tiny amount of Prussian blue can colour a vast quantity of paint. It is transparent to semi-transparent, making it excellent for glazing techniques, and it produces beautiful dark blues, blue-blacks, and (when mixed with yellow) vivid greens that no previous pigment could match.

SAFETY WARNING: The synthesis involves potassium ferrocyanide, which is itself of low toxicity, but releases hydrogen cyanide (HCN) gas if heated above 300°C or treated with strong acid. The reaction also uses iron sulfate (mildly irritating) and dilute hydrochloric acid. All steps must be performed in a well-ventilated area, and the reagents must NEVER be heated beyond the temperatures specified. Wear gloves, goggles, and a respirator when handling the acid. Dispose of all waste solutions responsibly.

Lengra kominn
2-3 hours active, overnight drying

Leiðbeiningar

1

Safety preparation

MANDATORY SAFETY: Work in a well-ventilated area — outdoors or under a fume hood. Put on chemical-resistant nitrile gloves, chemical splash goggles, and a P100/FFP3 respirator. The synthesis involves dilute hydrochloric acid (corrosive, produces HCl fumes) and potassium ferrocyanide (which releases hydrogen cyanide gas if overheated or exposed to strong acid). NEVER heat any solution above 60°C during this process. NEVER add concentrated acid to the ferrocyanide solution. Have clean water and baking soda available to neutralise any acid spills.

Nauðsynleg verkfæri:

Öndunargríma með síu fyrir sýrugufurÖndunargríma með síu fyrir sýrugufur
Hlífðargleraugu gegn efnaslettumHlífðargleraugu gegn efnaslettum
Efnaþolnir hanskarEfnaþolnir hanskar
2

Prepare the iron sulfate solution

Dissolve 25 g of ferrous sulfate (iron(II) sulfate, FeSO₄·7H₂O — also known as green vitriol or copperas) in 250 ml of warm water (40-50°C) in a glass beaker. Stir until completely dissolved. The solution should be a clear, pale green. Ferrous sulfate is the iron source — it provides the iron(II) ions that will form one half of the Prussian blue crystal structure. Use laboratory-grade or technical-grade ferrous sulfate — garden-variety iron sulfate may contain impurities that affect the pigment colour.

Efni fyrir þetta skref:

JárnsúlfatJárnsúlfat25 g

Nauðsynleg verkfæri:

Hitaþolinn glerbikarHitaþolinn glerbikar
HrærusprotiHrærusproti
Stafræn eldhúsvogStafræn eldhúsvog
3

Prepare the potassium ferrocyanide solution

In a separate clean glass beaker, dissolve 20 g of potassium ferrocyanide (K₄[Fe(CN)₆]·3H₂O — yellow prussiate of potash) in 250 ml of room-temperature water. Stir until completely dissolved. The solution should be a clear, bright yellow. SAFETY: Potassium ferrocyanide is of low toxicity in this form, but NEVER heat it above 300°C or mix it with strong acid — these conditions release hydrogen cyanide (HCN) gas, which is lethal. At room temperature in dilute solution, it is safe to handle with basic precautions (gloves, goggles).

Efni fyrir þetta skref:

KalíumferrósýaníðKalíumferrósýaníð20 g

Nauðsynleg verkfæri:

Bikarglas úr bórsílíkatiBikarglas úr bórsílíkati
4

Mix the two solutions to form the initial precipitate

Slowly pour the ferrous sulfate solution into the potassium ferrocyanide solution while stirring gently. A thick, dark blue-green precipitate forms immediately — this is 'Prussian white' (iron(II) ferrocyanide, also called Berlin white or Turnbull's blue precursor), which is actually a dark, greenish-blue at this stage. Stir thoroughly to ensure complete reaction. The mixture should be a thick, dark suspension with no clear yellow or green zones remaining. Let the precipitate settle for 15-20 minutes.

Nauðsynleg verkfæri:

TrésleifTrésleif
5

Oxidise with dilute hydrochloric acid to produce Prussian blue

The initial precipitate must be oxidised to convert it from the greenish intermediate to the vivid blue Prussian blue. Add 50 ml of dilute hydrochloric acid (10% HCl) slowly, stirring continuously. The acid serves two purposes: it acidifies the solution (promoting oxidation of Fe²⁺ to Fe³⁺ by dissolved oxygen) and helps develop the characteristic deep blue colour. As you add the acid, the precipitate shifts dramatically from dark greenish-blue to the brilliant, deep Prussian blue. Let the mixture stand, stirring occasionally, for 30-60 minutes to complete the oxidation. The supernatant liquid should become nearly clear as all the colour concentrates in the precipitate.

Efni fyrir þetta skref:

SaltsýraSaltsýra50 ml
6

Filter, wash, dry, and grind the finished pigment

Pour the blue precipitate through filter paper set in a funnel, collecting the clear filtrate below (dispose responsibly — it contains dissolved iron salts and traces of ferrocyanide). Wash the collected blue precipitate by pouring several portions of clean water through the filter — at least 500 ml total — to remove residual acid and salts. Unwashed Prussian blue tends to be unstable and can decompose over time. Once thoroughly washed, spread the wet pigment paste on a clean glass surface and let dry completely (1-3 days). The dried Prussian blue forms a hard, dark blue cake — grind to a fine powder with a glass muller. The finished pigment is an extraordinarily intense, transparent, deep blue. Store in a sealed glass jar away from strong light. Prussian blue is compatible with all painting binders and is especially valued in watercolour and oil for its intense tinting strength and transparency.

Nauðsynleg verkfæri:

SíupappírSíupappír
Trekt úr ryðfríu stáliTrekt úr ryðfríu stáli
GlerkvörnGlerkvörn
Glerkrukka með lokiGlerkrukka með loki

Efni

3

Nauðsynleg verkfæri

12

CC0 opinbert ríki

Þessi teikning er gefin út undir CC0. Þér er frjálst að afrita, breyta, dreifa og nota þetta verk í hvaða tilgangi sem er, án þess að biðja um leyfi.