PET Resin: Terephthalic Acid and Ethylene Glycol, Whinfield and Dickson

PET (polyethylene terephthalate) was invented by Whinfield and Dickson, whose patent (US 2,465,319, 1949) gives this first example: boil terephthalic acid in ethylene glycol until it dissolves, wash and dry the glycol ester, then heat it at 280 °C under nitrogen until it is a viscous polymer that melts at 254–255 °C and can be drawn into fibre. The melt is extruded and cut into chips (pellets) for moulding and spinning. The picture: our diagram.
Lengra kominn
About 4 days

Leiðbeiningar

1

Boil the acid in glycol

Reflux 50 g terephthalic acid with 89 g ethylene glycol for about 72 hours, until it has all dissolved. This makes glycol terephthalate.

Efni fyrir þetta skref:

TereftalsýraTereftalsýra50 g
EtýlenglýkólEtýlenglýkól89 g

Nauðsynleg verkfæri:

SkálavogSkálavog
KúlukolbaKúlukolba
EimsvalaspírallEimsvalaspírall
HitaplataHitaplata
2

Wash and dry the ester

Wash the glycol terephthalate with water and dry it under vacuum.

Nauðsynleg verkfæri:

Eimað vatnEimað vatn
Glertrekt með stútGlertrekt með stút
SíupappírSíupappír
LofttæmidælaLofttæmidæla
3

Heat at 280 °C under nitrogen

Melt it and heat at 280 °C for 8½ hours in a slow stream of nitrogen: no air may reach it. It grows thick as it polymerises.

Nauðsynleg verkfæri:

KúlukolbaKúlukolba
HitaplataHitaplata
Hitanemapar með aflestriHitanemapar með aflestri
KöfnunarefnishylkiKöfnunarefnishylki
Hitaþolnir hanskarHitaþolnir hanskar
Hlífðargleraugu gegn efnaslettumHlífðargleraugu gegn efnaslettum
4

Test for cold-drawing

Pull a thread from the melt with a rod and let it cool. It is ready when the cold thread can be stretched to several times its length. The finished polymer melts at 254–255 °C.

Nauðsynleg verkfæri:

GlerhrærusprotiGlerhrærusproti
Hitaþolnir hanskarHitaþolnir hanskar
5

Extrude and cut into chips

Extrude the molten polymer, let it cool, and cut it into chips (pellets).

Nauðsynleg verkfæri:

PlastþrýstivélPlastþrýstivél
KögglunarvélKögglunarvél
Hitaþolnir hanskarHitaþolnir hanskar

Efni

2

Nauðsynleg verkfæri

15

Tengd Blueprint

Þessi blueprint deila þekkingu — tækni, efni eða meginreglur

CC0 opinbert ríki

Þessi teikning er gefin út undir CC0. Þér er frjálst að afrita, breyta, dreifa og nota þetta verk í hvaða tilgangi sem er, án þess að biðja um leyfi.

Studdu smiðinn með því að kaupa vörur í gegnum teikningu hans þar sem hann fær þóknun smiða sem seljendur ákvarða, eða búðu til nýja endurskoðun á þessari teikningu og tengdu hana sem tengingu í þinni eigin teikningu til að deila tekjum.

Umræða

(0)

Skrá inn til að taka þátt í umræðunni

Hleður athugasemdum...