The dark grey ceramic magnet on fridges and in loudspeakers is barium ferrite. It is made from two cheap powders: one part barium carbonate to six of iron oxide, milled, fired, milled again, pressed and sintered. No cobalt or nickel is needed. This is Example 34 of the Philips patent. This iteration sinters at 1300 °C, where his rod held 1,850 gauss with a coercive force of 1,780 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956). They pressed rods; the claim covers "a body of a desired shape", and the disc size is ours. The patent does not say how to magnetise it; our way is stated. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Avanzato
2 days

Istruzioni

1

Weigh one part barium carbonate to six of iron oxide

Weigh 39.5 g of barium carbonate (0.2 mol) and 191.7 g of ferric oxide, Fe2O3 (1.2 mol). Barium carbonate is poisonous if swallowed: ours, gloves and a dust respirator.

Materiali per questo passaggio:

Carbonato di bario (witherite)Carbonato di bario (witherite)39.5 g
Ossido ferricoOssido ferrico191.7 g

Strumenti necessari:

Bilancia a bracciBilancia a bracci
Guanti di gommaGuanti di gomma
Respiratore P100Respiratore P100
2

Mill with ethanol for 4 hours

Grind the mixture with ethanol in an iron ball mill for 4 hours. Let the ethanol evaporate, then dry the powder in a drying oven.

Strumenti necessari:

Mulino a sfere di ferroMulino a sfere di ferro
Etanolo per laboratorio, 95 %Etanolo per laboratorio, 95 %
EssiccatoioEssiccatoio
3

Presinter at 1000 °C for 4 hours

Fire the dry powder in air at 1000 °C for 4 hours (ours: in a lidded porcelain crucible in a muffle furnace). Let it cool.

Strumenti necessari:

Forno a muffolaForno a muffola
Crogiolo con coperchio (porcellana)Crogiolo con coperchio (porcellana)
Tenaglia per crogioloTenaglia per crogiolo
Guanti resistenti al caloreGuanti resistenti al calore
4

Mill again for 4 hours

Grind the presintered product with ethanol in the ball mill for another 4 hours. Let the ethanol evaporate.

Strumenti necessari:

Mulino a sfere di ferroMulino a sfere di ferro
Etanolo per laboratorio, 95 %Etanolo per laboratorio, 95 %
EssiccatoioEssiccatoio
Respiratore P100Respiratore P100
5

Press discs at 1.5 tons per cm²

Press the powder at 1.5 tons/cm². The patent pressed rods; we press discs. Ours: a die 20 mm across, so about 4.7 tonnes on the punch (our arithmetic: 1.5 × 3.14 cm²).

Strumenti necessari:

Pressa idraulicaPressa idraulica
Stampo per pressatura di dischiStampo per pressatura di dischi
6

Sinter 4 hours at 1300 °C

Sinter the discs for 4 hours at 1300 °C in oxygen or in air. The patent's rod at 1300 °C: 1,850 gauss and 1,780 oersted.

Strumenti necessari:

Forno a muffolaForno a muffola
Tenaglia per crogioloTenaglia per crogiolo
Guanti resistenti al caloreGuanti resistenti al calore
7

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

Strumenti necessari:

ElettromagneteElettromagnete
BussolaBussola

Materiali

2

Strumenti richiesti

14

Questo progetto realizza

CC0 Pubblico dominio

Questo progetto è rilasciato sotto CC0. Sei libero di copiare, modificare, distribuire e utilizzare quest'opera per qualsiasi scopo, senza chiedere permesso.

Supporta il Maker acquistando prodotti tramite il suo progetto dove guadagna una Commissione Maker stabilita dai venditori, oppure crea una nuova iterazione di questo progetto e includilo come collegamento nel tuo progetto per condividere i ricavi.

Commenti

(0)

Accedi per partecipare alla discussione

Caricamento commenti...