Butyl Rubber
Polyisobutylene was a soft, sticky material that could not be vulcanised - it had no double bonds left for sulphur to bridge. At Standard Oil in 1937 William Sparks and Robert Thomas added a few percent of isoprene to the isobutylene, just enough double bonds to cure it, and polymerised the mix far below freezing. The result held air better than any rubber before it, and inner tubes have been made of it ever since.
**US 2,356,128**, "Mixed olefinic polymerization process and product", Thomas and Sparks, assigned to Jasco, filed 20. October 1939, granted 22. August 1944: an isoolefin with a small amount of diolefin, polymerised below 0 °C (down to about -160 °C) with aluminium chloride; it describes "a low, controlled, chemical unsaturation, capable of being cured with sulfur".
**You measure the two properties that made its name**: it barely bounces, and it barely leaks.
Principiante
1 hour plus a week of readings
Istruzioni
1
1
Make a butyl pad
Make a butyl pad
Cut 80 mm pieces from a bicycle inner tube and flatten them. Stack three (six walls) and tape the edges so it is about as thick as the natural rubber sheet.
Materiali per questo passaggio:
Camera d'aria1 pezzo
Nastro di carta per mascherature1 rotoloStrumenti necessari:
Forbici2
2
Drop and watch
Drop and watch
Tape a metal ruler upright beside each pad on a solid floor. Drop the steel ball from 500 mm, five times per pad, and read the top of the first bounce. Filming at eye level makes it easier.
Materiali per questo passaggio:
Lastra di gomma naturale1 pezzoStrumenti necessari:
Cuscinetto a sfere in acciaio
Riga metallica3
3
Inflate the leak test
Inflate the leak test
Pump the rest of the tube just until it is round - do not stretch it. Blow up a latex balloon to about the same firmness and tie it. Mark where you will measure each with tape.
Materiali per questo passaggio:
Palloncini1 confezioneStrumenti necessari:
Pompa a pedale per bicicletta4
4
Measure for a week
Measure for a week
Each day at the same time measure the balloon round its middle and the tube round its cross-section at the mark. Note the room temperature.
Strumenti necessari:
Metro a nastro
Termometro da ambiente5
5
Bounce and leak
Bounce and leak
Caricamento del notebook Jupyter…
6
6
History & Context
History & Context
**What the patent specifies:** isobutylene with a little conjugated diolefin, polymerised below 0 °C with aluminium chloride in an alkyl halide, then sulphur-cured. **Modern build (derived):** a commercial butyl inner tube.
Butyl became a strategic wartime rubber, then the air-holding liner inside every tubeless tyre, plus pond liners, roof membranes and engine mounts. Its limits: it is slow to vulcanise, does not bond well to other rubbers, and swells in oil and petrol.
Materiali
4- 1 pezzoSegnaposto
- 1 rotoloSegnaposto
- 1 pezzoSegnaposto
- 1 confezioneSegnaposto
Strumenti richiesti
6- Segnaposto
- Segnaposto
- Segnaposto
- Segnaposto
- 1 vendor sell this, none ship to you yetSegnaposto
- Segnaposto
Blueprint correlati
Questi blueprint condividono conoscenze — tecniche, materiali o principi
CC0 Pubblico dominio
Questo progetto è rilasciato sotto CC0. Sei libero di copiare, modificare, distribuire e utilizzare quest'opera per qualsiasi scopo, senza chiedere permesso.
Supporta il Maker acquistando prodotti tramite il suo progetto dove guadagna una Commissione Maker stabilita dai venditori, oppure crea una nuova iterazione di questo progetto e includilo come collegamento nel tuo progetto per condividere i ricavi.