Ferrite Toroid Core: Magnesium-Zinc Ferrite (28 : 18 : 54) Fired at 1400 °C (Snoek)
Charlie

Creato da

Charlie

21. ottobre 2026DE
2
0
0
0
0

Ferrite Toroid Core: Magnesium-Zinc Ferrite (28 : 18 : 54) Fired at 1400 °C (Snoek)

Ferrite is a ceramic magnet: iron oxide combined with other metal oxides, carrying magnetic flux while hardly conducting electricity. In his first ferrite patent (US 2,452,529, 1948) Snoek at Philips ground the oxides very fine and fired rings in oxygen. This magnesium-zinc ferrite (28 : 18 : 54 mol %) is milled 30 hours and fired 2 hours at 1400 °C; his core had an initial permeability of 150. The picture: our diagram.
Avanzato
3 days

Istruzioni

1

Mix 28 : 18 : 54 mol

Mix pure magnesium oxide, zinc oxide and ferric oxide, 28 : 18 : 54 mol %. Ours, by weight: 10.06 g magnesium oxide, 13.06 g zinc oxide and 76.88 g ferric oxide per 100 g.

Materiali per questo passaggio:

Ossido di magnesioOssido di magnesio10.06 g
Polvere di ossido di zincoPolvere di ossido di zinco13.06 g
Ossido ferricoOssido ferrico76.88 g

Strumenti necessari:

Bilancia a bracciBilancia a bracci
Mascherina antipolvereMascherina antipolvere
2

Grind 30 hours in an iron ball mill

Grind the mixture for 30 hours in an iron ball mill.

Strumenti necessari:

Mulino a sfere di ferroMulino a sfere di ferro
Mascherina antipolvereMascherina antipolvere
3

Mould a ring at 4 tons per cm²

Press the powder at 4 tons per square centimetre into a ring 3 cm across with a 4 × 4 mm section.

Strumenti necessari:

Pressa idraulicaPressa idraulica
Stampo di pressatura ad anelloStampo di pressatura ad anello
4

Fire 2 hours at 1400 °C, cool slowly

Heat the ring in oxygen for 2 hours at 1400 °C, then cool it slowly in oxygen at 5–10 °C a minute. Snoek's core: initial permeability 150.

Strumenti necessari:

Forno a tuboForno a tubo
OssigenoOssigeno
Bombola di gas in pressioneBombola di gas in pressione
PirometroPirometro
Tenaglia per crogioloTenaglia per crogiolo
Guanti resistenti al caloreGuanti resistenti al calore

Materiali

3

Strumenti richiesti

11

CC0 Pubblico dominio

Questo progetto è rilasciato sotto CC0. Sei libero di copiare, modificare, distribuire e utilizzare quest'opera per qualsiasi scopo, senza chiedere permesso.

Supporta il Maker acquistando prodotti tramite il suo progetto dove guadagna una Commissione Maker stabilita dai venditori, oppure crea una nuova iterazione di questo progetto e includilo come collegamento nel tuo progetto per condividere i ricavi.

Commenti

(0)

Accedi per partecipare alla discussione

Caricamento commenti...