Iron hydroxide is thrown down from hot ferric nitrate solution with ammonia, washed, dried and calcined. All of it ends as pure hematite, but the colour moves from bright red through dark red to purple as the calcining heat rises from 1000 °C, because the grains grow larger and more crystalline. Result: pure violet to purple ferric oxide (hematite) after 4 hours at 1000-1100 °C. Source: Nurdini et al., Heliyon 8 (2022) e10377, sections 2.2 and 4. Not given: batch size, how much ammonia, end pH, yield. Picture drawn by Youblob.
Intermedio
2 days

Istruzioni

1

Heat the ferric nitrate solution

Make a 0.05 M solution of ferric nitrate in distilled water and heat it to 80 °C.

Materiali per questo passaggio:

Nitrato ferricoNitrato ferrico1 as required

Strumenti necessari:

Acqua distillataAcqua distillata
Becher di vetroBecher di vetro
Piastra riscaldantePiastra riscaldante
TermometroTermometro
2

Throw down the hydroxide with ammonia

Keeping it at 80 °C, add ammonia solution drop by drop while stirring well. Stir for 3 hours, then let it cool to room temperature: a red-brown precipitate forms. Not given: how much ammonia.

Strumenti necessari:

Soluzione di ammoniaca al 25-28 %Soluzione di ammoniaca al 25-28 %
Imbuto gocciolatoreImbuto gocciolatore
Piastra riscaldantePiastra riscaldante
TermometroTermometro
3

Spin down, wash and dry

Collect the precipitate in a centrifuge at 4000 rpm for 15 minutes, wash it with distilled water, and dry it at 110 °C for 24 hours.

Strumenti necessari:

Centrifuga da bancoCentrifuga da banco
Acqua distillataAcqua distillata
EssiccatoioEssiccatoio
4

Calcine at 1000-1100 °C

Calcine for 4 hours in air at 1000-1100 °C. Below 1000 °C it stays bright or dark red; from 1000 °C it turns purple. Grind the cooled oxide to a fine powder (they used an agate mortar).

Strumenti necessari:

Forno a muffolaForno a muffola
Mortaio e pestelloMortaio e pestello

Materiali

1

Strumenti richiesti

10

CC0 Pubblico dominio

Questo progetto è rilasciato sotto CC0. Sei libero di copiare, modificare, distribuire e utilizzare quest'opera per qualsiasi scopo, senza chiedere permesso.