Pierre Castan, a Swiss chemist at the dental firm De Trey Frères, was looking for a resin for dentures. He reacted a phenol carrying two hydroxy groups with epichlorohydrin, then hardened the product with an acid anhydride, and got a hard, clear, unusually adherent solid. Ciba licensed it and sold it as Araldite; in the US Sylvan Greenlee developed epoxies independently. **US 2,324,483**, "Process of preparing synthetic resins", Castan, granted 20. July 1943, claims condensing "a polybasic carboxylic acid anhydride" with the product of "a phenol having at least two phenolic hydroxy groups and of an epichlorhydrine". It does not single out bisphenol A, the phenol most epoxies use today. **Epichlorohydrin is a carcinogen; you start from a two-part kit.** You glue pine lap joints at the right ratio and four wrong ones, then test hardness and break the joints.
初心者
2 hours plus 24 h cure

手順

1

Cut the joint pieces

Saw ten pine strips 100 x 25 mm. Sand one face of each end with 120 grit and dust off. Label five pairs 1:1, 1.25:1, 1:1.25, 1.5:1 and 1:1.5.

このステップの材料:

松板松板1
紙やすり紙やすり1
マスキングテープマスキングテープ1

必要な工具:

手のこぎり手のこぎり
鋼尺鋼尺
鉛筆鉛筆
2

Measure by syringe

Gloves on. For each ratio draw resin and hardener in separate syringes (1:1 = 2 ml + 2 ml; 1.25:1 = 2.5 + 2; and so on) into its own cup. This assumes a 1:1-by-volume kit - scale to your label.

このステップの材料:

二液性エポキシ二液性エポキシ25 ml

必要な工具:

ニトリル手袋ニトリル手袋
注射器セット注射器セット
目盛付き混合カップ目盛付き混合カップ
透明保護メガネ透明保護メガネ
3

Mix thoroughly

Stir each cup 2 minutes, scraping the walls and bottom. Unmixed streaks behave like a wrong ratio.

必要な工具:

撹拌棒撹拌棒
4

Glue and pour

Spread each mix on the sanded ends of its pair, overlap them 25 mm and spring-clamp over wax paper. Pour the rest as a coin-sized puddle on wax paper beside it.

このステップの材料:

ワックスペーパーワックスペーパー1

必要な工具:

バネクランプバネクランプ
5

Cure 24 hours

Leave everything at room temperature, 20 °C or warmer, for 24 hours. Cold slows the cure.
6

Pencil hardness

Sharpen pencils 6B to 6H and flatten the tips on 400 grit. Push each at 45° across a puddle, from hard down, until one no longer scratches. Record that grade.

必要な工具:

鉛筆セット(黒鉛)鉛筆セット(黒鉛)
拡大ルーペ拡大ルーペ
7

Break the joints

Clamp one strip of a joint in the vise and tap the free end sideways with the mallet until it breaks. Estimate how much of the bond face is torn wood.

必要な工具:

万力(ベンチバイス)万力(ベンチバイス)
ゴムハンマーゴムハンマー
透明保護メガネ透明保護メガネ
8

Ratio, leftovers, results

Jupyter ノートブックを読み込み中…
9

History & Context

**What the patent specifies:** a resin from a two-hydroxy phenol and epichlorohydrin, hardened by a polybasic acid anhydride. **Modern build (derived):** a two-part kit, most with an amine hardener that cures at room temperature. Epoxy became the glue that holds metal, the matrix of fibreglass and carbon-fibre parts, and the boat-builder's resin. Its limits: it yellows in sunlight, softens with heat, and uncured resin and hardener sensitise skin - which is why the gloves stay on every time.

材料

5

必要な工具

13

CC0 パブリックドメイン

このブループリントはCC0で公開されています。許可を求めずに、自由にコピー、修正、配布、あらゆる目的で使用できます。

メイカーを応援するには、ブループリント経由で製品を購入してください。メイカーには メイカーコミッション がベンダーにより設定されています。または、このブループリントの新しいイテレーションを作成し、自分のブループリントにコネクションとして含めて収益を共有できます。

ディスカッション

(0)

ログイン してディスカッションに参加

コメントを読み込み中...