Cyanoacrylate Adhesive
Woody

作成者

Woody

22. 9月 2026NO
49
0
0
0
0

Cyanoacrylate Adhesive

Harry Coover first met cyanoacrylates in 1942 while looking for a clear plastic for gun sights, and rejected them because they stuck to everything. In 1951 at Eastman Kodak he and Fred Joyner met them again - and this time saw a glue that set in seconds with no heat or pressure. It was sold from 1958. **US 2,794,788**, "Adhesive compositions containing alkyl esters of cyanoacrylic acid", Coover and Shearer, Eastman Kodak, filed 1. November 1952, granted 4. June 1957, claims the monomeric alkyl α-cyanoacrylate adhesive. **US 2,768,109**, "Alcohol-catalyzed alpha-cyanoacrylate adhesive compositions", Coover, filed 2. June 1954, granted 23. October 1956, claims "strongly bonding wood having an acidic surface character" by first moistening it with an alcohol of 1 to 8 carbon atoms. **You test that second claim on oak**, an acidic wood: dry, wiped with isopropyl alcohol, and misted with water.
初心者
1 hour plus 24 h

手順

1

Cut the strips

Saw eighteen oak strips 80 x 20 mm, about 5 mm thick. Sand one end face of each with 180 grit and dust off. Pencil-mark three groups: dry, IPA, water.

このステップの材料:

ホワイトオークの板ホワイトオークの板1 個

必要な工具:

手のこぎり手のこぎり
紙やすり紙やすり
2

Prepare the surfaces

Leave the first group dry. Wipe the ends of the second with isopropyl alcohol on a towel and use them within a minute. Give the third one light mist of water and blot. Note the room humidity.

必要な工具:

霧吹き霧吹き
湿度計湿度計
ペーパータオルペーパータオル
イソプロピルアルコール 99 %イソプロピルアルコール 99 %
3

Glue and time

Gloves and glasses on. One drop of CA on one end, overlap a partner strip by 20 mm, press 5 seconds and start the stopwatch. Every 10 seconds hang the spring scale from the free strip and pull to 2 N: record when it first holds. Three joints per group.

必要な工具:

ストップウォッチストップウォッチ
ばねばかり(力計)ばねばかり(力計)
ニトリル手袋ニトリル手袋
透明保護メガネ透明保護メガネ
瞬間接着剤(シアノアクリレート)瞬間接着剤(シアノアクリレート)
4

Break them tomorrow

After 24 hours clamp one strip of each joint in the vise and tap the free end sideways with the mallet until it breaks. Estimate how much of the bond area is torn wood.

必要な工具:

万力(ベンチバイス)万力(ベンチバイス)
ゴムハンマーゴムハンマー
透明保護メガネ透明保護メガネ
5

Set times and joints

Jupyter ノートブックを読み込み中…
6

History & Context

**What the patents specify:** a monomeric alkyl α-cyanoacrylate adhesive held liquid by an acid inhibitor, and, for acidic surfaces, a prior wipe with a C1–C8 alcohol. **Modern build (derived):** hardware-store CA glue on oak. CA spread from industry to every workshop, and in the Vietnam War medics used a CA spray to seal wounds; purpose-made medical grades followed. Its limits: brittle joints that fail in peel and impact, poor gap filling, and it bonds skin instantly - acetone releases it.
ステップ 6 - Image 1

材料

1

必要な工具

13

関連ブループリント

これらのブループリントは知識を共有しています — 技術、材料、原理

CC0 パブリックドメイン

このブループリントはCC0で公開されています。許可を求めずに、自由にコピー、修正、配布、あらゆる目的で使用できます。

メイカーを応援するには、ブループリント経由で製品を購入してください。メイカーには メイカーコミッション がベンダーにより設定されています。または、このブループリントの新しいイテレーションを作成し、自分のブループリントにコネクションとして含めて収益を共有できます。

ディスカッション

(0)

ログイン してディスカッションに参加

コメントを読み込み中...