Rotational Moulding: No Pressure At All

Every other process in this batch pushes polymer somewhere: a screw rams it, air inflates it, a haul-off drags it. Rotational moulding pushes nothing. Powder is weighed into a cold mould, the mould is closed and tumbled about two axes inside an oven, and the powder melts and sticks to the inside surface wherever it touches. Because there is no pressure, there is no clamping force, no core, no ejection system and no injection unit — so the tool can be cast aluminium or fabricated sheet and costs a small fraction of an injection mould. Water tanks, kayaks, road barriers, playground equipment and fuel tanks are made this way, seamless and stress-free. The price is time. This rung works out both sides of that bargain, and makes a small part with an oven and a hand-turned frame.
中級者
About 3 hours

手順

1

Find the signature of a rotomoulded part

Rotomoulded parts announce themselves once you know what to look for. Find a water butt, a kayak, a wheelie bin, a road barrier or a large planter and examine it. - **No parting line worth the name** across the body, and **no gate**. There is a mould split, but nothing was injected anywhere. - **Generous radii everywhere.** Powder will not flow into a sharp internal corner; it bridges. A rotomoulded part has no sharp corners at all, and a designer who draws one gets a thin spot. - **The wall is thicker at the corners**, which is the exact opposite of rung 3's blow moulding. Nothing was stretched, so powder simply collected where it had more surface to sit against. - **A slightly textured or matt inside surface**, and often a faint pebbling, because the last powder to melt never fully levelled. - **No internal stress.** Squeeze it, cut it, drill it — it does not spring or craze the way an injection moulding does, because nothing was forced anywhere. Cut a sample if you can, and measure the wall at a flat, a corner and a boss. Write the three numbers down; step 4's arithmetic predicts the flat one from the charge weight.

必要な工具:

デジタルノギス 6インチデジタルノギス 6インチ
マイクロメータマイクロメータ
クラフトナイフクラフトナイフ
デジタル顕微鏡デジタル顕微鏡
定規定規
透明保護メガネ透明保護メガネ
実験ノート(複写式)実験ノート(複写式)
2

Rotomould something small

The process scales down honestly, and a small oven plus a hand-turned frame is enough to make a real part. **The mould.** Two aluminium halves that clamp together — a simple sphere or a rounded box, 60–100 mm across — with a small vent hole so the air inside can expand and escape. Every rotomould has a vent; without one the pressure inside pushes the melt away from the wall and the part comes out thin and bubbled. **The charge.** Weigh polyethylene powder into the mould. Step 4 gives the arithmetic; for a 80 mm sphere aiming at a 2 mm wall you want roughly 40 g. Use **powder**, not pellets: pellets do not melt evenly at these temperatures and leave a lumpy, porous wall. If you only have pellets, grind them cold. **The rotation.** Two axes, slowly, at different speeds — a common ratio is about 4:1 between the major and minor axes, which is what stops the powder tracing the same path twice. A simple hand frame with two cranks is perfectly adequate for a small part, and turning it by hand for twenty minutes teaches you more about the process than any description. **The heat.** Oven at about 250–280 °C for polyethylene, and the number that matters is the **internal air temperature** rather than the oven setting. Keep turning throughout. You are done when the inside surface has gone glossy — in a production machine an air probe reports this; on the bench, judge by time and then by the result. **The cool.** Keep turning while it cools or the melt slumps to the bottom. Cool slowly with air; quenching a rotomoulded part warps it badly, because the wall is thick and the polymer is semi-crystalline. An oven at 280 °C and a hot metal mould that must be handled while turning. Leather gloves rated for heat, a face shield, a stable frame, and ventilation — polyethylene above about 300 °C degrades and the fumes are genuinely harmful. Do not exceed the temperature and do not leave it unattended.

このステップの材料:

回転成形用ポリエチレン粉末回転成形用ポリエチレン粉末1 個
アルミ板(6061-T6)アルミ板(6061-T6)1 個

必要な工具:

オーブントースターオーブントースター
赤外線温度計赤外線温度計
MAX6675 モジュール付き K 型熱電対MAX6675 モジュール付き K 型熱電対
デジタルスケールデジタルスケール
万力(ベンチバイス)万力(ベンチバイス)
ボール盤ボール盤
やすり(手やすり)やすり(手やすり)
革の作業用手袋革の作業用手袋
フェイスシールドフェイスシールド
透明保護メガネ透明保護メガネ
ドラフトチャンバー(排気ダクト式)ドラフトチャンバー(排気ダクト式)
消火器消火器
ストップウォッチストップウォッチ
実験ノート(複写式)実験ノート(複写式)
3

Make the three classic faults happen

Three faults account for most of what goes wrong, and each has an unmistakable appearance. Produce all three deliberately and keep the samples. **Bubbles (under-cooked).** Take the part out early. The wall is full of trapped air between partly-fused powder grains, and it looks like frozen foam in section. This is the commonest real fault: the powder melted and stuck but never coalesced. The fix is more time at temperature, not more temperature. **Degradation (over-cooked).** Leave one in too long. The inside surface goes yellow or brown and the part becomes brittle; it may smell. Polyethylene oxidises from the inside surface outward because that is where the hot air is. Note that the outside can look perfect. **Warping (cooled wrong).** Quench one in cold water. It will distort, and it will keep distorting for hours as stresses relax. Compare with one air-cooled slowly on the frame. Section all three plus a good one, and look at the wall under the microscope. The good part has a uniform, dense, slightly glossy inner face. The under-cooked one is porous. The over-cooked one is discoloured at the inner face specifically. Then break each one. Under-cooked parts fail at a fraction of the load because every bubble is a void, and this is the reason rotomoulding is judged on internal air temperature rather than on the clock.

このステップの材料:

回転成形用ポリエチレン粉末回転成形用ポリエチレン粉末1 個

必要な工具:

オーブントースターオーブントースター
赤外線温度計赤外線温度計
MAX6675 モジュール付き K 型熱電対MAX6675 モジュール付き K 型熱電対
デジタル顕微鏡デジタル顕微鏡
クラフトナイフクラフトナイフ
ばねばかり(力計)ばねばかり(力計)
ストップウォッチストップウォッチ
革の作業用手袋革の作業用手袋
フェイスシールドフェイスシールド
透明保護メガネ透明保護メガネ
ドラフトチャンバー(排気ダクト式)ドラフトチャンバー(排気ダクト式)
実験ノート(複写式)実験ノート(複写式)
4

Charge weight, wall thickness and where the energy goes

Jupyter ノートブックを読み込み中…

必要な工具:

デジタルスケールデジタルスケール
5

History and context

**Attribution, stated honestly.** No patent is asserted here. Rotational moulding of hollow objects is very old — rotating a mould containing a liquid to coat its inside is how chocolate shells and hollow metal castings were already being made in the nineteenth century, and the catalogue's slip casting rung is the same idea in ceramics. The plastics version arrives with **polyethylene powder** in the 1950s, and the process was developed across the industry rather than by a single filing. **What it is actually for.** Not speed, and not precision. Rotomoulding wins on three things nothing else offers together: **very low tool cost**, so short runs and large parts are affordable; **seamless, stress-free hollow parts** with no weld line and no ejection marks; and **uniform corners**, because powder collects rather than stretches. A 1,000 litre water tank is a rotomoulding because no other process could make one at all without joining pieces. **The comparison worth holding.** Injection moulding puts the cost in the tool and almost none in the cycle. Rotational moulding puts almost none in the tool and all of it in the cycle. Step 4's energy split is why: most of the heat goes into the mould, and it all has to come out again before the part can be removed. **Honest limits.** Cycle times of twenty minutes to an hour, so labour and energy per part are high. Tolerances are poor — plus or minus several per cent on wall — and wall thickness cannot be varied deliberately except by adding insulation to the mould. No sharp corners, no fine detail, no threads worth having. The polymer choice is narrow because the powder must sinter and flow at oven temperature without degrading, which in practice means polyethylene for the overwhelming majority of parts. And the process is genuinely hot and genuinely slow, which is why step 2 is written with as much space given to the gloves as to the powder.

材料

2

必要な工具

20

CC0 パブリックドメイン

このブループリントはCC0で公開されています。許可を求めずに、自由にコピー、修正、配布、あらゆる目的で使用できます。

メイカーを応援するには、ブループリント経由で製品を購入してください。メイカーには メイカーコミッション がベンダーにより設定されています。または、このブループリントの新しいイテレーションを作成し、自分のブループリントにコネクションとして含めて収益を共有できます。

ディスカッション

(0)

ログイン してディスカッションに参加

コメントを読み込み中...