Silver Solder from Fine Silver, Copper and Spelter: Gee, 1877

Silver solder joins silver, copper and brass with a strong, hard seam. The silversmith George Gee preferred one made of fine silver, shot copper and a little spelter (zinc), melted only once: his best hard solder is 16 dwt of fine silver, 3 dwt 12 gr of shot copper and 12 gr of spelter to the ounce, about 80, 17.5 and 2.5 per cent. More copper and zinc make it flow sooner (his medium, easy and common solders). Silver and copper alone give the hardest, least fusible solder; too much zinc makes it eat away during soldering.
中級者
Two hours

手順

1

Weigh the metals

Jupyter ノートブックを読み込み中…

このステップの材料:

純銀純銀80 g
銅インゴット銅インゴット17.5 g
亜鉛インゴット亜鉛インゴット2.5 g

必要な工具:

はかりはかり
たがねたがね
2

Anneal and test the crucible

Before a new plumbago (graphite) crucible is charged, heat it slowly to redness on a fire that is dying down and has no blaze, so it does not crack. Touch it with a cold iron bar: if cracks show, reject it.

必要な工具:

黒鉛粘土坩堝黒鉛粘土坩堝
木炭炉木炭炉
るつぼばさみるつぼばさみ
3

Melt silver and copper

Put the copper at the bottom of the crucible, the silver on top, and melt them in the furnace. Stir them well together with an iron stirrer, tapered at the point and first heated to redness. When the metals are just beginning to fuse, cover the melt with finely divided, pure charcoal to keep the air off it.

このステップの材料:

木炭 - 細かく砕いたもの木炭 - 細かく砕いたもの1 as required

必要な工具:

木炭炉木炭炉
鉄製撹拌棒鉄製撹拌棒
耐熱手袋耐熱手袋
4

Add the spelter

Hold the spelter in a long pair of tongs over the mouth of the crucible, inside the furnace, until it has almost reached its melting point, then drop it into the molten metal and stir quickly so it mixes in. Zinc burns away quickly in the air, so it goes in last.

必要な工具:

火ばさみ火ばさみ
鉄製撹拌棒鉄製撹拌棒
耐熱手袋耐熱手袋
5

Pour the ingot

Withdraw the crucible from the furnace at once and pour into an ingot mould that is clean, smooth, lightly greased, dusted with fine charcoal and warmed: a cold mould makes the metal spout, but do not overheat it either. Melt solder only once; Gee found that solders containing volatile metals grow hard, brittle and drossy with repeated melting.

このステップの材料:

木炭 - 細かく砕いたもの木炭 - 細かく砕いたもの1 as required

必要な工具:

るつぼばさみるつぼばさみ
インゴット鋳型インゴット鋳型
耐熱手袋耐熱手袋
6

Roll into pallions or file to dust

Roll the solder out thin between flattening rollers and cut it lengthways and then crossways with hand shears into little bits (pallions), or file it into fine dust, according to the work in hand. The work is then bound together, wetted with a paste of borax and water, and the pallions laid on the joints and melted with a blowpipe flame.

必要な工具:

圧延機(ローリングミル)圧延機(ローリングミル)
金切り鋏金切り鋏
やすり(手やすり)やすり(手やすり)

材料

4

必要な工具

12

この設計図で作るもの

CC0 パブリックドメイン

このブループリントはCC0で公開されています。許可を求めずに、自由にコピー、修正、配布、あらゆる目的で使用できます。

メイカーを応援するには、ブループリント経由で製品を購入してください。メイカーには メイカーコミッション がベンダーにより設定されています。または、このブループリントの新しいイテレーションを作成し、自分のブループリントにコネクションとして含めて収益を共有できます。

ディスカッション

(0)

ログイン してディスカッションに参加

コメントを読み込み中...