Butt-weld steel pipe, 1/8 to 3 inches, as National Tube made it in 1921: hot skelp is pulled by tongs and a draw-bench chain through a bell a little larger than the finished pipe, which curls it into a tube and presses its edges together into a weld. The pipe is then rolled to size, straightened, cleaned, threaded and pressure-tested. Each length, 20 to 40 ft, is welded in one pull. Every pipe is tested inside at 700 to 800 lb per square inch. Source: National Tube Co., "National" Modern Welded Pipe (1921), pp. 41-47. Picture: drawing butt-weld pipe.
上級者
Unknown

手順

1

Heat the skelp

Charge the skelp from the rear into a long welding furnace, a little longer than the skelp, with a narrow opening at each end, and bring it to welding heat.

このステップの材料:

鋼スケルプ(管用帯鋼)鋼スケルプ(管用帯鋼)1 one piece per length of pipe

必要な工具:

溶接炉溶接炉
2

Draw it through the bell

Grip the trimmed end with long-handled tongs and pull it through a die, or bell, slightly larger than the finished pipe. Hook the tongs to the travelling chain of the draw bench, which pulls the whole length (20 to 40 ft) through. The skelp is a little wider than the bell's inside circumference, so it curls into a tube and its edges butt squarely and weld. Some sizes go through two bells at one heat, the second slightly smaller.

必要な工具:

引抜台(ドローベンチ)引抜台(ドローベンチ)
鍛冶ばさみ(やっとこ)鍛冶ばさみ(やっとこ)
溶接炉溶接炉
3

For Double Extra Strong pipe

Thick skelp needs so great a pull that a strong bar is welded on its end as a 'bait' for the tongs. Draw it several times through bells of decreasing size, reheating between draws, so the seam is thoroughly welded.

必要な工具:

引抜台(ドローベンチ)引抜台(ドローベンチ)
鍛冶ばさみ(やっとこ)鍛冶ばさみ(やっとこ)
溶接炉溶接炉
4

Size and round

Pass the pipe through sizing rolls, which reduce it slightly, lengthen it and loosen the heavy welding scale. Then roll it to its finished size and circular shape, which removes the scale and leaves the walls smooth.

必要な工具:

圧延機(ローリングミル)圧延機(ローリングミル)
5

Cool, straighten and clean

Let the pipe cool slowly as it crosses a table, then straighten and smooth it in cross rolls. Wash off the loosened scale in a tank; blow it out of the smaller sizes with compressed air.

必要な工具:

圧延機(ローリングミル)圧延機(ローリングミル)
水水
空気圧縮機空気圧縮機
6

Cut, thread and test

Cut off a short length at each end, where the tong jaws crushed it. Thread the pipe, then test it inside with water at 700 to 800 lb per square inch to prove the wall and the weld. Ours: hacksaw, die set and hand test pump; the booklet does not say how the ends are cut or threaded.

必要な工具:

金切りのこ(ハクソー)金切りのこ(ハクソー)
ねじ切りタップダイスセットねじ切りタップダイスセット
手動水圧テストポンプ手動水圧テストポンプ

材料

1

必要な工具

9

CC0 パブリックドメイン

このブループリントはCC0で公開されています。許可を求めずに、自由にコピー、修正、配布、あらゆる目的で使用できます。

メイカーを応援するには、ブループリント経由で製品を購入してください。メイカーには メイカーコミッション がベンダーにより設定されています。または、このブループリントの新しいイテレーションを作成し、自分のブループリントにコネクションとして含めて収益を共有できます。

ディスカッション

(0)

ログイン してディスカッションに参加

コメントを読み込み中...