Guitar Strings: Bronze Wound on Steel, Then Heat-Soaked (Stone and Falcone 1977)
A wound string is a steel core with another wire wrapped round it. Stone and Falcone believed the wrap keeps stresses from the winding and slowly unwinds as the string is played, so the tone goes dead. Their fix: after winding, heat-soak the string, at least 2 hours at 270 °F or 30 minutes at 480 °F for a bronze wrap, then let it cool.
Source: W. N. Stone and A. S. Falcone (National Musical String Co.), US 4,063,674 (1977). Unknown: where phosphor bronze wire comes from, and the gauges. The winding, which the patent calls conventional, is ours, after Landtroop and Dykstra, US 6,256,872 (2001). These are linked to unknown heads. The plain strings of the set are steel music wire; that, the oven and the nitrogen are ours. Picture drawn by Youblob.
上級者
1 day
手順
1
1
Cut the core and plain strings
Cut the core and plain strings
Cut steel music wire for the cores of the wound strings and for the plain strings of the set. Unknown: the gauges and lengths, and the ball ends.
このステップの材料:
鋼製ピアノ線 0.032 インチ1 as required必要な工具:
ニッパー
不明な寸法2
2
Wind the bronze wrap at room temperature
Wind the bronze wrap at room temperature
Wrap phosphor bronze wire helically round each core at room temperature. The patent prefers a wrap that expands more with heat than the core. The patent says only 'in a conventional manner'. Ours, after Landtroop and Dykstra, US 6,256,872 (2001): hook the core's ball end on the motor-driven headstock spindle, grip the other end in the tailstock chuck and stretch it with the tailstock tension cylinder; fix the end of the cover wire at the ball end, then spin the core while a carriage travels toward the tailstock, paying the cover wire out under tension from its spool; cut it off at the end.
このステップの材料:
リン青銅線1 as required必要な工具:
弦巻線機
不明な寸法
保護めがね3
3
Heat-soak the wound strings
Heat-soak the wound strings
Heat the wound strings for a bronze wrap at 270-480 °F (132-249 °C): at least 2 hours at 270 °F or at least 30 minutes at 480 °F, shorter the hotter. If the wire tarnishes in hot air, do it without air, in nitrogen or carbon dioxide. The wrap's turns settle into more even spacing.
必要な工具:
オーブン
実験用温度計
窒素ガスボンベ4
4
Cool and set up the set
Cool and set up the set
Let the strings cool back to room temperature. Make up the set with the plain steel strings.
必要な工具:
ニッパー関連ブループリント
これらのブループリントは知識を共有しています — 技術、材料、原理
CC0 パブリックドメイン
このブループリントはCC0で公開されています。許可を求めずに、自由にコピー、修正、配布、あらゆる目的で使用できます。
メイカーを応援するには、ブループリント経由で製品を購入してください。メイカーには メイカーコミッション がベンダーにより設定されています。または、このブループリントの新しいイテレーションを作成し、自分のブループリントにコネクションとして含めて収益を共有できます。