Ushirikiano
SANAA
UREMBO NA USTAWI
UJANJA
UTAMADUNI NA HISTORIA
BURUDANI
MAZINGIRA
CHAKULA NA VINYWAJI
UHANDISI WA KINYUME
SAYANSI
MICHEZO
TEKNOLOJIA
VAZI
Violet Iron Oxide: Precipitated Hematite Calcined at 1000-1100 °C (Nurdini et al. 2022)
Charlie

Imeundwa na

Charlie

1. Novemba 2026DE
13
0
0
0
0

Violet Iron Oxide: Precipitated Hematite Calcined at 1000-1100 °C (Nurdini et al. 2022)

Iron hydroxide is thrown down from hot ferric nitrate solution with ammonia, washed, dried and calcined. All of it ends as pure hematite, but the colour moves from bright red through dark red to purple as the calcining heat rises from 1000 °C, because the grains grow larger and more crystalline. Result: pure violet to purple ferric oxide (hematite) after 4 hours at 1000-1100 °C. Source: Nurdini et al., Heliyon 8 (2022) e10377, sections 2.2 and 4. Not given: batch size, how much ammonia, end pH, yield. Picture drawn by Youblob.
Kati
2 days

Maagizo

1

Heat the ferric nitrate solution

Make a 0.05 M solution of ferric nitrate in distilled water and heat it to 80 °C.

Vifaa kwa hatua hii:

Nitrati ya feriNitrati ya feri1 as required

Zana zinazohitajika:

Maji yaliyosafishwa kwa mvukeMaji yaliyosafishwa kwa mvuke
Bikari ya kiooBikari ya kioo
Sahani ya Kupasha JotoSahani ya Kupasha Joto
KipimajotoKipimajoto
2

Throw down the hydroxide with ammonia

Keeping it at 80 °C, add ammonia solution drop by drop while stirring well. Stir for 3 hours, then let it cool to room temperature: a red-brown precipitate forms. Not given: how much ammonia.

Zana zinazohitajika:

Myeyusho wa amonia - asilimia 25-28Myeyusho wa amonia - asilimia 25-28
Funeli ya kudondoshaFuneli ya kudondosha
Sahani ya Kupasha JotoSahani ya Kupasha Joto
KipimajotoKipimajoto
3

Spin down, wash and dry

Collect the precipitate in a centrifuge at 4000 rpm for 15 minutes, wash it with distilled water, and dry it at 110 °C for 24 hours.

Zana zinazohitajika:

Kizungushi cha mezaKizungushi cha meza
Maji yaliyosafishwa kwa mvukeMaji yaliyosafishwa kwa mvuke
Tanuri la kukaushiaTanuri la kukaushia
4

Calcine at 1000-1100 °C

Calcine for 4 hours in air at 1000-1100 °C. Below 1000 °C it stays bright or dark red; from 1000 °C it turns purple. Grind the cooled oxide to a fine powder (they used an agate mortar).

Zana zinazohitajika:

Tanuri ya muffleTanuri ya muffle
Kinu na mchiKinu na mchi

Vifaa

1

Zana Zinazohitajika

10

CC0 Umma Wote

Mchoro huu umetolewa chini ya CC0. Uko huru kunakili, kubadilisha, kusambaza, na kutumia kazi hii kwa madhumuni yoyote, bila kuomba ruhusa.

Saidia Mtengenezaji kwa kununua bidhaa kupitia Mchoro wao ambapo wanapata Kamisheni ya Mtengenezaji iliyowekwa na Wachuuzi, au unda marudio mapya ya Mchoro huu na uiunganishe kama kiungo katika Mchoro wako kuchangia mapato.

Majadiliano

(0)

Ingia kujiunga na majadiliano