PTFE Thread Seal Tape: Paste-Extruded, Calendered, Never Sintered
The white tape wound on pipe threads is PTFE that has never been melted. Fine PTFE powder is mixed with a lubricant, pressed into a slug, squeezed through a slit die by a ram, rolled thin between two rolls, and dried. Kept below the sintering heat (about 350 °C) it stays soft and conforms to the thread (process: US 5,415,939, 1995). The targets and tests are those of the Indian standard IS 14643 (from BS 4375): no fillers, at most 0.1 % lubricant left, usually 12 mm wide and 0.075 mm thick.
The lubricant (naphtha) and the slitter are ours. The picture: Fig. 1a of the patent.
កម្រិតខ្ពស់
1 day
ការណែនាំ
1
1
Wet the powder
Wet the powder
Mix fine (dispersion-made) virgin PTFE powder with a lubricant that can be driven off completely. Granular PTFE will not paste-extrude. No fillers. Ours: naphtha, as required.
សម្ភារៈសម្រាប់ជំហាននេះ៖
ម្សៅ PTFE ល្អិត1 batchឧបករណ៍ដែលត្រូវការ៖
ណាហ្វ្តា2
2
Press a preform
Press a preform
Compact the wet powder into a cylindrical preform in a mould with a plunger.
ឧបករណ៍ដែលត្រូវការ៖
ពុម្ពសង្កត់
ម៉ាស៊ីនសង្កត់អ៊ីដ្រូលិក3
3
Ram-extrude a flat tape
Ram-extrude a flat tape
Put the preform in the extrusion press. The plunger pushes it out through a slit die as a thick flat tape.
ឧបករណ៍ដែលត្រូវការ៖
ម៉ាស៊ីនសង្កត់ច្របាច់អ៊ីដ្រូលិក4
4
Calender it thin
Calender it thin
Pass the tape between two counter-rotating rolls to a thin tape, aiming at about 0.075 mm.
ឧបករណ៍ដែលត្រូវការ៖
ម៉ាស៊ីនរមៀលលោហៈ
មីក្រូម៉ែត្រ5
5
Dry off the lubricant
Dry off the lubricant
Dry the tape until the lubricant is gone. Keep it well below the sintering heat (about 350 °C): sintered tape is stiff and will not seal.
ឧបករណ៍ដែលត្រូវការ៖
ឡសម្ងួត6
6
Slit and spool
Slit and spool
Slit it to width, usually 12 mm (±0.5 mm), and wind it on spools.
ឧបករណ៍ដែលត្រូវការ៖
ម៉ាស៊ីនកាត់ និងរុំឡើងវិញ7
7
Check the tape
Check the tape
It must look white, with no visible specks or torn edges. Measure the thickness at five points along a sample; each must be within 10 % of their mean.
ឧបករណ៍ដែលត្រូវការ៖
មីក្រូម៉ែត្រ8
8
Test the residual lubricant
Test the residual lubricant
Weigh about 15 g of tape. Extract it in a Soxhlet with petroleum spirit (40-60 °C) for at least 4 h, dry it at 100 °C, then heat it at 300 °C for 6 h, cool and weigh. The loss must be 0.1 % or less.
ឧបករណ៍ដែលត្រូវការ៖
ឧបករណ៍ស្រង់សុកស្លេត
អេទែរប្រេងកាត
ឡសម្ងួត
ឆ្នាំងរំលាយដែក
បន្ទប់សម្ងួត (តូច)
ជញ្ជីងល្អិត9
9
Wrap a thread
Wrap a thread
Wind tape round an R 1/2 taper pipe thread with 50 % overlap, two layers deep, just tight enough to take the thread form. It must hold the form, not break, and its end must stay put.
ឧបករណ៍ដែលត្រូវការ៖
គ្រឿងតភ្ជាប់បំពង់មានខ្សែវីសសម្ភារៈ
1- 1 batchកន្លែងទុក
ឧបករណ៍ចាំបាច់
14- កន្លែងទុក
- កន្លែងទុក
- កន្លែងទុក
- កន្លែងទុក
- កន្លែងទុក
- កន្លែងទុក
- កន្លែងទុក
- កន្លែងទុក
- កន្លែងទុក
- កន្លែងទុក
- កន្លែងទុក
- កន្លែងទុក
- កន្លែងទុក
- កន្លែងទុក
ប្លង់ពាក់ព័ន្ធ
ប្លង់ទាំងនេះចែករំលែកចំណេះដឹង — បច្ចេកទេស សម្ភារៈ ឬគោលការណ៍
CC0 សាធារណៈ
ប្លង់នេះត្រូវបានចេញផ្សាយក្រោម CC0។ អ្នកមានសិទ្ធិចម្លង កែប្រែ ចែកចាយ និងប្រើប្រាស់ដោយមិនចាំបាច់សុំអនុញ្ញាត។
គាំទ្រអ្នកបង្កើតដោយទិញផលិតផលតាមរយៈប្លង់របស់ពួកគេ ដែលពួកគេទទួលបាន កម្រៃជើងសារអ្នកបង្កើត កំណត់ដោយអ្នកលក់ ឬបង្កើតកំណែថ្មីនៃប្លង់នេះ ហើយបញ្ចូលជាការតភ្ជាប់ក្នុងប្លង់របស់អ្នកដើម្បីចែករំលែកចំណូល។